{"id":61723,"date":"2017-01-20T14:00:36","date_gmt":"2017-01-20T06:00:36","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=61723"},"modified":"2017-03-04T17:15:12","modified_gmt":"2017-03-04T09:15:12","slug":"avd-mater-%ef%bc%9a3d%e6%89%93%e5%8d%b0%e5%af%bc%e7%94%b5%e6%b0%b4%e5%87%9d%e8%83%b6%e5%bc%b9%e6%80%a7%e4%bd%93","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=61723","title":{"rendered":"Adv. Mater.\uff1a3D\u6253\u5370\u5bfc\u7535\u6c34\u51dd\u80f6\u5f39\u6027\u4f53"},"content":{"rendered":"<p>\u3010\u5f15\u8bed\u3011<\/p>\n<p>\u8fd1\u5e74\u6765\uff0c\u67d4\u6027\u7535\u5b50\u4ea7\u54c1\u7684\u5e94\u7528\u65e5\u6108\u706b\u70ed\uff0c\u6bd4\u5982\u4eba\u4f53\u53ef\u7a7f\u6234\u4f20\u611f\u5668\u3001\u8f6f\u4f53\u673a\u5668\u4eba\u4e2d\u7684\u53cd\u9988\u4f20\u611f\u5668\u3002\u8fd9\u5bf9\u67d4\u6027\u6750\u6599\u53c8\u63d0\u51fa\u4e86\u65b0\u7684\u8981\u6c42\u2014\u2014\u9700\u8981\u5728\u4fdd\u6301\u9ad8\u5e94\u53d8\u7684\u6761\u4ef6\u4e0b\uff0c\u4ecd\u80fd\u591f\u5728\u5404\u79cd\u73af\u5883\u4e0b\u4fdd\u6301\u529f\u80fd\u6027\u3002\u4f46\u73b0\u5b58\u7684\u6750\u6599\uff0c\u5927\u591a\u90fd\u65e0\u6cd5\u5728\u4fdd\u6301\u9ad8\u7684\u5bfc\u7535\u7387\u548c\u62c9\u4f38\u6027\u7684\u540c\u65f6\u62e5\u6709\u5149\u5b66\u900f\u660e\u5ea6\uff0c\u5bfc\u81f4\u5176\u5728\u5149\u5b66\u9886\u57df\u7684\u5e94\u7528\u53d7\u963b\u3002\u4f7f\u7528\u5177\u6709\u9ad8\u5f39\u6027\u548c\u900f\u660e\u5ea6\u7684\u51dd\u80f6\u4f5c\u4e3a\u5bfc\u4f53\u5236\u5907\u7535\u8def\u88c5\u7f6e\uff0c\u6b63\u6210\u4e3a\u4e00\u79cd\u8d8a\u6765\u8d8a\u53d7\u6b22\u8fce\u7684\u65b9\u5f0f\u3002\u5bfc\u7535\u6027\u51dd\u80f6\u901a\u5e38\u5206\u4e3a\u6c34\u51dd\u80f6\u548c\u79bb\u5b50\u51dd\u80f6\uff0c\u76f8\u6bd4\u8f83\u800c\u8a00\uff0c\u79bb\u5b50\u51dd\u80f6\u4e0d\u4f1a\u8131\u6c34\uff0c\u4f46\u662f\u6bd4\u6c34\u51dd\u80f6\u5bfc\u7535\u6027\u7a0d\u900a\u4e00\u7b79\uff0c\u540c\u65f6\u79bb\u5b50\u6db2\u4e5f\u4f1a\u5e72\u6270\u4e00\u4e9b\u51dd\u80f6\u7684\u805a\u5408\u53cd\u5e94\u3002\u6c34\u51dd\u80f6\u66f4\u5bb9\u6613\u5408\u6210\uff0c\u4f46\u662f\u6613\u8131\u6c34\uff0c\u589e\u52a0\u5b83\u7684\u79bb\u5b50\u5bfc\u7535\u7387\u548c\u4fdd\u6c34\u6027\uff0c\u540c\u65f6\u4fdd\u8bc1\u5176\u5e73\u8861\u4ee5\u8fbe\u5230\u6700\u597d\u7684\u6548\u679c\u3002<\/p>\n<p>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/p>\n<p>\u9488\u5bf9\u8fd9\u7c7b\u6c34\u51dd\u80f6\u7684\u5236\u5907\uff0c\u54c8\u4f5b\u5927\u5b66\u7684Joost J. Vlassak\u548cZhigang Suo\uff08\u5171\u540c\u901a\u8baf\u4f5c\u8005\uff09\u8bfe\u9898\u7ec4\u8fd1\u65e5\u5728Advanced Materails\u4e0a\u53d1\u8868\u4e86\u4e00\u7bc7\u540d\u4e3a\u201c3D Printing of Transparent and Conductive Heterogeneous Hydrogel\u2013Elastomer Systems\u201d\u7684\u6587\u7ae0\uff0c\u62a5\u544a\u4e86\u4f7f\u75283D\u6253\u5370\u7684\u65b9\u5f0f\uff0c\u5370\u5237\u51fa\u4e00\u79cd\u96c6\u6210\u4e86\u5bfc\u7535\u6c34\u51dd\u80f6\u548c\u4ecb\u7535\u5f39\u6027\u4f53\u7684\u67d4\u6027\u53ef\u62c9\u4f38\u7684\u7535\u5b50\u5668\u4ef6\u3002\u8fd9\u4e24\u79cd\u6750\u6599\u90fd\u53ef\u4ee5\u5206\u522b\u96c6\u6210\u4e8e\u88c5\u7f6e\u4e0a\u3002\u5c06\u4ed6\u4eec\u4e00\u8d77\u6253\u5370\u540e\uff0c\u6d4b\u5f97\u6750\u6599\u540c\u65f6\u62e5\u6709\u826f\u597d\u7684\u673a\u68b0\u6027\u80fd\u548c\u7535\u5b66\u6027\u80fd\uff0c\u5e76\u4e14\u6253\u5370\u51fa\u4e00\u4e2a\u8f6f\u5e94\u53d8\u4f20\u611f\u5668\uff0c\u8bc1\u5b9e\u4e86\u8be5\u6253\u5370\u65b9\u5f0f\u7684\u53ef\u884c\u6027\u3002\u8be5\u5668\u4ef6\u7684\u6750\u6599\u4e3a\u805a\u4e19\u70ef\u9170\u80fa\uff08PAAm\uff09\u6c34\u51dd\u80f6\u548c\u805a\u4e8c\u7532\u57fa\u7845\u6c27\u70f7\uff08PDMS\uff09\uff0c\u4e24\u79cd\u6750\u6599\u90fd\u5177\u6709\u826f\u597d\u7684\u7535\u5b66\u548c\u5149\u5b66\u6027\u80fd\u3002<\/p>\n<p>[\u81f4\u6b49\uff1a\u5f88\u62b1\u6b49\u901a\u8baf\u4f5c\u8005Zhigang Suo\u7684\u786e\u5207\u4e2d\u6587\u540d\u6ca1\u6709\u627e\u5230\uff0c\u5c0f\u7f16\u5728\u6b64\u8868\u793a\u8bda\u631a\u7684\u6b49\u610f\uff01]<\/p>\n<p>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/p>\n<p>\u56fe1\uff1a3D\u6253\u5370\u7cfb\u7edf\u603b\u4f53\u793a\u610f\u56fe<\/p>\n<p><span style=\"color: #000000;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-61727\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/1_\u526f\u672c.png\" alt=\"\" width=\"700\" height=\"334\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/1_\u526f\u672c.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/1_\u526f\u672c-300x143.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/span><\/p>\n<p>a)\u4f7f\u75283D\u6253\u5370\u673a\u8fdb\u884c\u5370\u5237\uff0c\u5305\u62ec\u7cbe\u5bc6\u5b9a\u4f4d\u7cfb\u7edf\uff0c\u6cb9\u58a8\u6324\u51fa\u7cfb\u7edf\u548c\u786c\u4ef6\/\u8f6f\u4ef6\u63a5\u53e3\uff0c\u53ef\u4ee5\u7cbe\u786e\u63a7\u5236\u6750\u6599\u5728\u6837\u54c1\u53f0\u4e0a\u7684\u6324\u51fa\u4f4d\u7f6e\u548c\u901f\u7387\u3002<\/p>\n<p>b\uff09\u5e76\u6392\u6bd4\u8f83\u539f\u59cb\u8bbe\u7f6e\u7684\u56fe\u6848\u548c\u5b9e\u9645\u6253\u51fa\u7684\u6548\u679c\u3002<\/p>\n<p>c\uff09\u900f\u660e\u5ea6\u7684\u5c55\u793a\uff0c\u7528\u76f8\u540c\u7684\u6750\u6599\u6253\u5370\u4e86\u4e00\u4e2a\u5177\u6709\u900f\u660e\u7ed3\u6784\u7684\u56fe\u6848\u3002<\/p>\n<p><strong>\u56fe2\uff1a\u6c34\u51dd\u80f6\u524d\u805a\u4f53\u6eb6\u6db2\u7684\u6d41\u53d8\u6027\u5206\u6790<\/strong><\/p>\n<p><span style=\"color: #000000;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-61728\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/2_\u526f\u672c.png\" alt=\"\" width=\"700\" height=\"239\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/2_\u526f\u672c.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/2_\u526f\u672c-300x102.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/span><\/p>\n<p>a)\u5178\u578b\u7684\u632f\u8361\u6d41\u53d8\u7ed3\u679c\uff0c\u663e\u793a\u51fa\u968f\u7740\u526a\u5207\u5e94\u529b\u7684\u589e\u52a0\uff0c\u6cb9\u58a8\u7684\u526a\u5207\u5b58\u50a8\uff08G\u2019\uff09\u548c\u524d\u5207\u635f\u5931\uff08G\u201d\uff09\u7684\u53d8\u5316\u8d8b\u52bf\u3002\u50a8\u80fd\u6a21\u91cf\uff08G\u2019\uff09\u5728558.5\u00b14.6Pa\u4e4b\u524d\u4fdd\u6301\u7a33\u5b9a\uff0c\u5e76\u5728570 Pa\u4e4b\u524d\u9ad8\u4e8e\u635f\u8017\u6a21\u91cf\uff08G\u201d\uff09\uff0c\u5728\u5927\u4e8e570Pa\u7684\u5e94\u529b\u4e0b\uff0cG\u201d\u8d85\u8fc7G\u2019\uff0c\u6b64\u65f6\u7269\u8d28\u7684\u72b6\u6001\u4e3a\u7c98\u7a20\u6db2\u4f53\u3002<\/p>\n<p>b)\u5178\u578b\u7684\u7c98\u5ea6\u6d4b\u5b9a\u7ed3\u679c\uff0c\u663e\u793a\u51fa\u968f\u7740\u526a\u5207\u901f\u7387\u7684\u53d8\u5316\uff0c\u7c98\u5ea6\u548c\u5e94\u529b\u7684\u8d8b\u52bf\u3002\u7531\u8be5\u66f2\u7ebf\u53ef\u89c1\u6750\u6599\u6709\u660e\u663e\u7684\u526a\u5207\u53d8\u7a00\u6548\u5e94\u3002<\/p>\n<p><strong>\u56fe3\uff1a\u6c34\u51dd\u80f6\u7684\u6253\u5370\u7a0b\u5e8f\u8bbe\u8ba1<\/strong><\/p>\n<p>&nbsp;<\/p>\n<p><span style=\"color: #000000;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-61729\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/3_\u526f\u672c.png\" alt=\"\" width=\"700\" height=\"364\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/3_\u526f\u672c.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/3_\u526f\u672c-300x156.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/span><\/p>\n<p>a)\u5728\u6a2a\u5411\uff08x\uff09\u548c\u7eb5\u5411(z)\u6253\u5370\u51fa\u5404\u79cd\u6c34\u51dd\u80f6\u7ebf\u51e0\u4f55\u5f62\u72b6\u793a\u610f\u56fe\u3002<\/p>\n<p>b\u3001c\uff09\u7cbe\u786e\u8bbe\u5b9aX\u8f74\u548cZ\u8f74\u4e0a\u7684\u8be6\u7ec6\u7ebf\u6570\uff0c\u5c06\u6c34\u51dd\u80f6\u6253\u5370\u5728PDMS\u4e0a\u3002<\/p>\n<p>d~f)\u591a\u5c42\u51dd\u80f6\u56fe\u6848\u7684\u5149\u5b66\u663e\u5fae\u56fe\u50cf\uff0c\u663e\u793a\u4e86\u5e73\u6ed1\u7684\u5408\u5e76\u754c\u9762\u548c\u7531\u6c34\u51dd\u80f6\u8fb9\u7f18\u7684\u6b8b\u7559\u6da6\u6e7f\u5c42\u3002<\/p>\n<p>g\u3001h\uff09\u4f7f\u7528\u5149\u5b66\u8f6e\u5ed3\u6d4b\u5b9a\u6cd5\u83b7\u5f97\u5370\u5237\u7684\u6c34\u51dd\u80f6\u7ebf\u7684\u6a2a\u622a\u9762\u56fe\uff0c\u53d1\u73b0\u8fd9\u4e9b\u8f6e\u5ed3\u51e0\u4e4e\u662f\u76f8\u540c\u7684\uff0c\u8868\u660e\u5176\u8bbe\u8ba1\u7684\u6c34\u51dd\u80f6\u53ef\u4ee5\u91cd\u590d\u5370\u5236\u3002<\/p>\n<p><strong>\u56fe4\uff1a\u6240\u5f97\u6c34\u51dd\u80f6\u7ed3\u6784\u7684\u7535\u5b66\u6027\u80fd\u6d4b\u8bd5<\/strong><\/p>\n<p>&nbsp;<\/p>\n<p><span style=\"color: #000000;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-61730\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/4_\u526f\u672c.png\" alt=\"\" width=\"700\" height=\"550\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/4_\u526f\u672c.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/4_\u526f\u672c-300x236.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><br \/>\n <\/span><\/p>\n<p>a\uff09\u7528\u56db\u70b9\u63a2\u9488\u6d4b\u91cf\u6cd5\u5f97\u5230\u7684I-V\u66f2\u7ebf\uff0c\u5757\u72b6\u6c34\u51dd\u80f6\u6837\u54c1\u5c3a\u5bf8\u5e73\u5747\u957f30cm\uff0c\u5bbd4.2mm\uff0c\u9ad83.5mm\u3002\u6b27\u59c6\u4f20\u5bfc\u7684\u7535\u5bfc\u7387\u4e3a10.39\u00b10.31S m-1\uff0c\u4e0e\u7528\u4e8e\u5bf9\u6bd4\u7684\u76d0\u6eb6\u6db2\u7535\u5bfc\u7387\u76f8\u5f53\u3002\u4f46\u662f\u6c34\u51dd\u80f6\u7ebf\u7535\u5bfc\u7387\u4e0b\u964d\uff0c\u8fd9\u4e0e\u5931\u6c34\u6709\u5173\u3002<\/p>\n<p>b\uff09PDMS\u886c\u5e95\u5370\u5237\u7684\u6c34\u51dd\u80f6\u5e76\u7ecf\u8fc7\u62c9\u4f38\u540e\u7684\u5f52\u4e00\u5316\u7535\u963b\u7edf\u8ba1\uff0c\u4e0e\u4e0d\u7ecf\u8fc7\u53d8\u5f62\u7684\u51e0\u4f55\u56fe\u6848\u76f8\u5bf9\u6bd4\u3002\u7167\u7247\u5bf9\u6bd4\u4e86\u6837\u54c1\u5728\u539f\u59cb\uff08\u5e94\u53d8= 0\uff05\uff09\u72b6\u6001\u548c\u62c9\u4f38\uff08\u5e94\u53d8= 50\uff05\uff09\u72b6\u6001\u7684\u7535\u963b\u3002\u8868\u660e\u5728\u8fd9\u4e2a\u5e94\u53d8\u4e0b\u6c34\u51dd\u80f6\u5b8c\u597d\u65e0\u635f\u3002<\/p>\n<p>c\uff09\u5370\u5237\u6c34\u51dd\u80f6\u7684\u75b2\u52b3\u5faa\u73af\u6570\u4e0e\u7535\u963b\u7684\u51fd\u6570\u3002\u8fdb\u884c20\uff05\u5e94\u53d8\u7684\u5355\u8f74\u62c9\u4f38\u5e94\u53d8\u5faa\u73af1000\u6b21\u3002\u5e76\u672a\u53d1\u73b0\u7535\u963b\u4ea7\u751f\u660e\u663e\u7684\u53d8\u5316\u3002\u6bd4\u8f83\u75b2\u52b3\u8bd5\u9a8c\u524d\u540e\u7684\u56fe\u50cf\uff0c\u5e76\u672a\u5f62\u6210\u53ef\u89c1\u7684\u635f\u4f24\u6216\u5206\u5c42\u3002<\/p>\n<p>d\uff09\u79bb\u5b50\u8f6c\u6362\u7387\u4e0e\u9891\u7387\u7ed8\u5173\u7cfb\u3002\u53ef\u4ee5\u89c2\u5bdf\u5230\u5b9e\u9a8c\u7ed3\u679c\u4e0e\u6587\u4e2d\u7406\u8bba\u7ed3\u679c\u7684\u62df\u5408\u5728\u4e00\u4e2a\u7406\u60f3\u7684\u6c34\u5e73\u3002<\/p>\n<p><strong>\u56fe5\uff1a\u6253\u5370\u7684\u5355\u56de\u8def\u7535\u963b\u5e94\u53d8\u4eea<\/strong><\/p>\n<p>&nbsp;<\/p>\n<p><span style=\"color: #000000;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-61731\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/5_\u526f\u672c.png\" alt=\"\" width=\"700\" height=\"382\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/5_\u526f\u672c.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/5_\u526f\u672c-300x164.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/span><span style=\"color: #000000;\">\u00a0<\/span><\/p>\n<p>&nbsp;<\/p>\n<p>a\uff09\u4f7f\u7528\u6c34\u51dd\u80f6\u4f5c\u4e3a\u5bfc\u4f53\u548cPDMS\u4f5c\u4e3a\u5c01\u88c5\u57fa\u5e95\u6765\u5236\u4f5c\u7684\u7b80\u5355\u7684\u57fa\u4e8e\u7535\u963b\u7684\u5e94\u53d8\u8ba1\u3002<\/p>\n<p>b\uff09\u901a\u8fc7\u5c06\u4f20\u611f\u5668\u8fde\u63a5\u5230\u67d4\u6027\u624b\u5957\u5e76\u5f2f\u66f2\u624b\u6307\uff0c\u6211\u4eec\u80fd\u591f\u89c2\u5bdf\u5230\u5728\u624b\u6307\u6700\u5927\u5f2f\u66f2\u65f6\uff0c\u4e0e\u521d\u59cb\u503c\u76f8\u6bd4\u7535\u963b\u53d8\u5316\u9ad8\u8fbe30\uff05\u3002<\/p>\n<p>c\uff09\u5c55\u793a\u4e86\u6bcf\u4e2a\u624b\u6307\u7684\u624b\u52bf\u53d8\u5316\u5f15\u8d77\u7684\u5e94\u53d8\u6240\u5bfc\u81f4\u5f97\u4f20\u611f\u5668\u7535\u963b\u968f\u7740\u65f6\u95f4\u7684\u53d8\u5316\u3002<\/p>\n<p>\u3010\u5c0f\u7ed3\u3011<\/p>\n<p>\u7efc\u4e0a\u6240\u8ff0\uff0c\u672c\u6587\u63cf\u8ff0\u4e86\u4e00\u79cd\u5bfc\u7535\u6c34\u51dd\u80f6\u7684\u5370\u5237\u65b9\u6cd5\u3002\u901a\u8fc7\u8c03\u8282\u6c34\u51dd\u80f6\u9884\u805a\u7269\u7684\u6d41\u53d8\u884c\u4e3a\u548c\u8fdb\u884cPDMS\u8868\u9762\u7684\u79bb\u5b50\u4f53\u5904\u7406\u540e\uff0c\u6253\u5370\u51fa\u538b\u6beb\u7c73\u7ea7\u7684\u57fa\u4e8e\u7535\u963b\u7684\u5e94\u53d8\u4f20\u611f\u5668\u3002\u5e76\u4e14\u53ef\u4ee5\u8bbe\u8ba1\u548c\u6253\u5370\u590d\u6742\u7684\u7ed3\u6784\uff0c\u8be5\u65b9\u5f0f\u53ef\u4ee5\u5e94\u7528\u548c\u4efb\u4f55PDMS-\u6c34\u51dd\u80f6\u6750\u6599\u4f53\u7cfb\u3002\u603b\u4e4b\uff0c\u672c\u6587\u63d0\u4f9b\u4e86\u4e00\u79cd\u7b80\u5355\u7684\u5236\u5907\u6c34\u51dd\u80f6\u548c\u7535\u89e3\u8d28\u5f39\u6027\u4f53\u7684\u65b9\u5f0f\uff0c\u53ef\u4ee5\u7528\u4e8e\u67d4\u6027\u7535\u6c14\u8bbe\u5907\u548c\u8f6f\u4f53\u673a\u5668\u4eba\u7b49\u9886\u57df\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1a<a href=\"http:\/\/onlinelibrary.wiley.com\/doi\/10.1002\/adma.201604827\/abstract\" target=\"_blank\">3D Printing of Transparent and Conductive Heterogeneous Hydrogel\u2013Elastomer Systems<\/a>\uff08Advanced Materails\uff0c2017, DOI: 10.1002\/adma.201604827\uff09<\/p>\n<p>\u8be5\u6587\u732e\u6c47\u603b\u7531\u6750\u6599\u4eba\u7f16\u8f91\u90e8\u675c\u5f81\u5ce5\u4f9b\u7a3f\uff0c\u6750\u6599\u725b\u7f16\u8f91\u6574\u7406\u3002<\/p>\n<p>\u6750\u6599\u4eba\u7f51\u4e13\u6ce8\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u53ca\u884c\u4e1a\u8fdb\u5c55\uff0c\u8fd9\u91cc\u6c47\u96c6\u4e86\u5404\u5927\u9ad8\u6821\u7855\u535a\u751f\u3001\u4e00\u7ebf\u79d1\u7814\u4eba\u5458\u4ee5\u53ca\u884c\u4e1a\u4ece\u4e1a\u8005\uff0c\u5982\u679c\u60a8\u5bf9\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u8fdb\u5c55\uff0c\u89e3\u8bfb\u9ad8\u6c34\u5e73\u6587\u7ae0\u6216\u662f\u8bc4\u8ff0\u884c\u4e1a\u6709\u5174\u8da3\uff0c\u70b9\u6211\u52a0\u5165\u7f16\u8f91\u90e8\u3002<\/p>\n<p>\u6750\u6599\u4eba\u7f51\u5411\u5404\u5927\u56e2\u961f\u8bda\u5fc3\u7ea6\u7a3f\uff0c\u8bfe\u9898\u7ec4\u6700\u65b0\u6210\u679c\u3001\u65b9\u5411\u603b\u7ed3\u3001\u56e2\u961f\u8bbf\u8c08\u3001\u5b9e\u9a8c\u6280\u80fd\u7b49\u7686\u53ef\u6295\u7a3f\uff0c\u8bf7\u8054\u7cfb\uff1a\u90ae\u7bb1tougao@cailiaoren.com \u6216 QQ\uff1a97482208\u3002<\/p>\n<p>\u4eea\u5668\u8bbe\u5907\u3001\u8bd5\u5242\u8017\u6750\u3001\u6750\u6599\u6d4b\u8bd5\u3001\u6570\u636e\u5206\u6790\uff0c\u627e\u6750\u6599\u4eba\u3001\u4e0a\u6d4b\u8bd5\u8c37\uff01<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8bed\u3011 \u8fd1\u5e74\u6765\uff0c\u67d4\u6027\u7535\u5b50\u4ea7\u54c1\u7684\u5e94\u7528\u65e5\u6108\u706b\u70ed\uff0c\u6bd4\u5982\u4eba\u4f53\u53ef\u7a7f\u6234\u4f20\u611f\u5668\u3001\u8f6f\u4f53\u673a\u5668\u4eba\u4e2d\u7684\u53cd\u9988\u4f20\u611f\u5668\u3002\u8fd9\u5bf9\u67d4\u6027\u6750\u6599\u53c8\u63d0\u51fa\u4e86\u65b0\u7684\u8981\u6c42\u2014\u2014\u9700\u8981\u5728\u4fdd\u6301\u9ad8\u5e94\u53d8\u7684\u6761\u4ef6\u4e0b\uff0c\u4ecd\u80fd\u591f\u5728&#8230;<\/p>\n","protected":false},"author":395,"featured_media":61746,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[28],"class_list":["post-61723","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-jiedu","tag-3d"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/61723"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/395"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=61723"}],"version-history":[{"count":18,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/61723\/revisions"}],"predecessor-version":[{"id":69463,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/61723\/revisions\/69463"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/61746"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=61723"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=61723"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=61723"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}