{"id":62661,"date":"2017-01-25T06:30:59","date_gmt":"2017-01-24T22:30:59","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=62661"},"modified":"2017-10-17T23:15:37","modified_gmt":"2017-10-17T15:15:37","slug":"%e5%ad%a6%e6%9c%af%e5%b9%b2%e8%b4%a7%e7%a2%b3%e7%ba%a4%e7%bb%b4%e5%a4%8d%e5%90%88%e6%9d%90%e6%96%99%e7%9a%84%e5%88%b6%e5%a4%87%e5%8f%8a%e5%85%b6%e4%ba%a7%e4%b8%9a%e5%ba%94%e7%94%a8","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=62661","title":{"rendered":"\u6280\u672f\u5e72\u8d27|\u78b3\u7ea4\u7ef4\u590d\u5408\u6750\u6599\u7684\u5236\u5907\u53ca\u5176\u4ea7\u4e1a\u5e94\u7528"},"content":{"rendered":"<p><span style=\"color: #0000ff;\"><strong>\u4e00\u3001 \u7b80\u4ecb<\/strong><\/span><br \/>\n\u78b3\u7ea4\u7ef4\u662f\u7ea4\u7ef4\u72b6\u7684\u78b3\u7d20\u6750\u6599\uff0c\u542b\u78b3\u91cf\u572890%\u4ee5\u4e0a\uff0c\u5b83\u662f\u5229\u7528\u5404\u79cd\u6709\u673a\u7ea4\u7ef4\u5728\u60f0\u6027\u6c14\u4f53\u4e2d\uff0c\u9ad8\u6e29\u72b6\u6001\u4e0b\u78b3\u5316\u800c\u5236\u5f97\u7684\u3002\u78b3\u7ea4\u7ef4\u5177\u6709\u5341\u5206\u4f18\u5f02\u7684\u529b\u5b66\u6027\u80fd\uff0c\u662f\u76ee\u524d\u5df2\u5927\u91cf\u751f\u4ea7\u7684\u9ad8\u6027\u80fd\u7ea4\u7ef4\u4e2d\u5177\u6709\u6700\u9ad8\u7684\u6bd4\u5f3a\u5ea6\u548c\u6700\u9ad8\u7684\u6bd4\u6a21\u91cf\u7684\u7ea4\u7ef4\uff0c\u7279\u522b\u662f\u57282000\uf0b0C\u4ee5\u4e0a\u7684\u9ad8\u6e29\u60f0\u6027\u73af\u5883\u4e2d\uff0c\u78b3\u7ea4\u7ef4\u662f\u552f\u4e00\u5f3a\u5ea6\u4e0d\u53d8\u7684\u7269\u8d28\uff0c\u662f\u5176\u4ed6\u4e3b\u8981\u7ed3\u6784\u6750\u6599\u6240\u65e0\u6cd5\u6bd4\u62df\u7684\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-62662\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/1-42.jpg\" alt=\"\" width=\"400\" height=\"246\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/1-42.jpg 400w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/1-42-300x185.jpg 300w\" sizes=\"(max-width: 400px) 100vw, 400px\" \/><br \/>\n\u4f5c\u4e3a\u9ad8\u6027\u80fd\u7ea4\u7ef4\u7684\u4e00\u79cd\uff0c\u78b3\u7ea4\u7ef4\u65e2\u6709\u78b3\u6750\u6599\u7684\u56fa\u6709\u7279\u6027\uff0c\u53c8\u517c\u5907\u4e86\u7eba\u7ec7\u7ea4\u7ef4\u7684\u67d4\u8f6f\u53ef\u52a0\u5de5\u6027\uff0c\u662f\u5148\u8fdb\u590d\u5408\u6750\u6599\u4e2d\u6700\u91cd\u8981\u7684\u589e\u5f3a\u6750\u6599\uff0c\u5df2\u7ecf\u5728\u519b\u4e8b\u4ee5\u53ca\u6c11\u7528\u4e2d\u7684\u5404\u4e2a\u9886\u57df\u53d6\u5f97\u5e7f\u6cdb\u5e94\u7528\u3002<\/p>\n<p>\u78b3\u7ea4\u7ef4\u590d\u5408\u6750\u6599\u662f\u4ee5\u78b3\u7ea4\u7ef4\u6216\u78b3\u7ea4\u7ef4\u7ec7\u7269\u4e3a\u589e\u5f3a\u4f53\uff0c\u6811\u8102\u4e3a\u57fa\u4f53\u6240\u5f62\u6210\u7684\u590d\u5408\u6750\u6599\uff0c\u82f1\u6587\u79f0\u4e4b\u4e3aCarbon Fiber-reinforced Polymer(CFRP)\u3002\u8fd9\u79cd\u6750\u6599\u5177\u6709\u5bc6\u5ea6\u4f4e\uff0c\u70ed\u81a8\u80c0\u7cfb\u6570\u5c0f\uff0c\u8010\u70e7\u8680\u6027\u80fd\u597d\uff0c\u8f7b\u8d28\u9ad8\u5f3a\u7b49\u4f18\u70b9\uff0c\u5177\u6709\u4f18\u5f02\u7684\u529b\u5b66\u6027\u80fd\u548c\u70ed\u7269\u7406\u6027\u80fd\uff0c\u4f7f\u5176\u88ab\u5e7f\u6cdb\u5e94\u7528\u4e8e\u519b\u4e8b\u3001\u822a\u7a7a\u3001\u4f53\u80b2\u7528\u54c1\u3001\u8d5b\u8f66\u7b49\u9886\u57df\uff0c\u53d1\u5c55\u6f5c\u529b\u5de8\u5927\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-62663\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/2-2-1.jpg\" alt=\"\" width=\"400\" height=\"276\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/2-2-1.jpg 400w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/2-2-1-300x207.jpg 300w\" sizes=\"(max-width: 400px) 100vw, 400px\" \/><\/p>\n<p><span style=\"color: #0000ff;\"><strong>\u4e8c\u3001 \u78b3\u7ea4\u7ef4\u590d\u5408\u6750\u6599\u7684\u7684\u5236\u5907<\/strong><\/span><\/p>\n<p><strong>1\u3001\u78b3\u7ea4\u7ef4\u7684\u751f\u4ea7<\/strong><\/p>\n<p>\u6839\u636e\u78b3\u7ea4\u7ef4\u539f\u6599\u7684\u4e0d\u540c\uff0c\u53ef\u4ee5\u5c06\u5176\u5206\u4e3a\u805a\u4e19\u70ef\u8148(PAN)\u57fa\u78b3\u7ea4\u7ef4\u3001\u6ca5\u9752\u57fa\u78b3\u7ea4\u7ef4\u3001\u7c98\u80f6\u57fa\u78b3\u7ea4\u7ef4\u3002<\/p>\n<p><strong>\uff081\uff09PAN\u57fa\u78b3\u7ea4\u7ef4<\/strong><\/p>\n<p>PAN\u57fa\u78b3\u7ea4\u7ef4\u5236\u9020\u7684\u7b2c\u4e00\u6b65\u662f\u7528\u4e19\u70ef\u8148(AN)\u5355\u4f53\u5236\u9020PAN\u539f\u4e1d\uff0c\u7b2c\u4e8c\u6b65\u662f\u539f\u4e1d\u7684\u9884\u6c27\u5316\u548c\u78b3\u5316\uff0c\u9884\u6c27\u5316\u5904\u7406\u7684\u76ee\u7684\u662f\u4f7fPAN\u7684\u7ebf\u6027\u5206\u5b50\u94fe\u8f6c\u5316\u4e3a\u8010\u70ed\u7684\u68af\u5f62\u7ed3\u6784\uff0c\u4f7f\u5176\u5728\u9ad8\u6e29\u4e0b\u78b3\u5316\u65f6\u4e0d\u7194\u4e0d\u71c3\uff0c\u4fdd\u6301\u7ea4\u7ef4\u5f62\u6001\u3002\u78b3\u5316\u8fc7\u7a0b\u662f\u78b3\u7ea4\u7ef4\u5f62\u6210\u7684\u4e3b\u8981\u9636\u6bb5\uff0c\u9664\u53bb\u4e86\u7ea4\u7ef4\u4e2d\u5927\u91cf\u7684\u6c27\u3001\u6c2e\u548c\u5176\u4ed6\u5143\u7d20\uff0c\u518d\u7ecf\u8fc7\u8868\u9762\u5904\u7406\u3001\u5e72\u71e5\u4e0a\u6d46\uff0c\u5f97\u5230\u5177\u6709\u91d1\u5c5e\u5149\u6cfd\u7684PAN\u57fa\u78b3\u7ea4\u7ef4\u4ea7\u54c1\u3002<\/p>\n<p><strong>\uff082\uff09\u6ca5\u9752\u57fa\u78b3\u7ea4\u7ef4<\/strong><\/p>\n<p>\u9996\u5148\u662f\u6ca5\u9752\u539f\u6599\u7684\u7cbe\u5236\uff0c\u4e3b\u8981\u662f\u4e3a\u4e86\u9664\u53bb\u6ca5\u9752\u4e2d\u7684\u6e38\u79bb\u70ad\u548c\u5176\u4ed6\u56fa\u4f53\u6742\u8d28\uff0c\u8fd9\u4e9b\u6742\u8d28\u518d\u7eba\u4e1d\u8fc7\u7a0b\u4e2d\u53ef\u80fd\u4f1a\u5835\u585e\u7eba\u4e1d\u5b54\uff0c\u63a5\u4e0b\u6765\u7684\u6ca5\u9752\u8c03\u5236\u8fc7\u7a0b\u662f\u901a\u8fc7\u6ca5\u9752\u7684\u70ed\u7f29\u805a\u3001\u52a0\u6c22\u9884\u5904\u7406\u3001\u6eb6\u5242\u8403\u53d6\u7684\u65b9\u6cd5\u5236\u53d6\u53ef\u7eba\u6ca5\u9752\uff0c\u76ee\u7684\u662f\u9664\u53bb\u6ca5\u9752\u4e2d\u7684\u8f7b\u7ec4\u5206\u3002\u6ca5\u9752\u7684\u7eba\u4e1d\u65b9\u6cd5\u4e3b\u8981\u53c8\u6324\u538b\u6cd5\u3001\u79bb\u5fc3\u6cd5\u3001\u7194\u5439\u6cd5\u3001\u6da1\u6d41\u6cd5\u7b49\u3002\u7531\u4e8e\u6ca5\u9752\u7684\u53ef\u6eb6\u6027\u548c\u7c98\u6027\uff0c\u5728\u521a\u5f00\u59cb\u52a0\u6e29\u5c31\u4f1a\u9ecf\u5408\u5728\u4e00\u8d77\uff0c\u800c\u4e0d\u80fd\u5f62\u6210\u5355\u4e1d\u7684\u78b3\u7ea4\u7ef4\uff0c\u6240\u4ee5\u5fc5\u987b\u5728\u78b3\u5316\u524d\u8fdb\u884c\u78b3\u7ea4\u7ef4\u7684\u9884\u6c27\u5316\u5904\u7406\u3002\u9884\u6c27\u5316\u5904\u7406\u8fd8\u53ef\u4ee5\u63d0\u9ad8\u6ca5\u9752\u7ea4\u7ef4\u7684\u529b\u5b66\u6027\u80fd\uff0c\u589e\u52a0\u78b3\u5316\u524d\u7684\u6297\u62c9\u5f3a\u5ea6\u3002\u9884\u6c27\u5316\u5904\u7406\u540e\u7684\u6ca5\u9752\u7ea4\u7ef4\u5c06\u5728\u60f0\u6027\u6c14\u4f53\u4e2d\u8fdb\u884c\u78b3\u5316\u6216\u77f3\u58a8\u5316\u5904\u7406\uff0c\u4ee5\u9664\u53bb\u5176\u4e2d\u7684\u975e\u78b3\u539f\u5b50\uff0c\u63d0\u9ad8\u529b\u5b66\u6027\u80fd\u3002<\/p>\n<p><strong>\uff083\uff09\u7c98\u80f6\u57fa\u78b3\u7ea4\u7ef4<\/strong><\/p>\n<p>\u7c98\u80f6\u57fa\u78b3\u7ea4\u7ef4\u4e3b\u8981\u7528\u4e8e\u8010\u70e7\u8680\u6750\u6599\u548c\u9694\u70ed\u6750\u6599\uff0c\u5176\u4ea7\u91cf\u4e0d\u8db3\u4e16\u754c\u78b3\u7ea4\u7ef4\u603b\u91cf\u76841%\uff0c\u4f46\u6709\u7740\u5176\u4ed6\u4e24\u79cd\u78b3\u7ea4\u7ef4\u4e0d\u53ef\u53d6\u4ee3\u7684\u5730\u4f4d\u3002\u751f\u4ea7\u7c98\u80f6\u57fa\u78b3\u7ea4\u7ef4\u7684\u539f\u6599\u4e3b\u8981\u662f\u6728\u6d46\u548c\u68c9\u6d46\uff0c\u7c98\u80f6\u7ea4\u7ef4\u6d46\u7c95\u914d\u5236\u6210\u7eba\u4e1d\u6db2\uff0c\u901a\u8fc7\u6e7f\u6cd5\u7eba\u5236\u6210\u7c98\u80f6\u8fde\u7eed\u957f\u4e1d\uff0c\u7c98\u80f6\u7ea4\u7ef4\u7ecf\u6c34\u6d17\u3001\u5e72\u71e5\u548c\u6d78\u6e0d\u50ac\u5316\u5242\u540e\uff0c\u518d\u7ecf\u9884\u6c27\u5316\u548c\u78b3\u5316\u5de5\u827a\u5c31\u53ef\u4ee5\u8f6c\u5316\u4e3a\u78b3\u7ea4\u7ef4\u3002<\/p>\n<p><strong>2\u3001\u78b3\u7ea4\u7ef4\u590d\u5408\u6750\u6599\u6210\u578b\u5de5\u827a<\/strong><\/p>\n<p>\u78b3\u7ea4\u7ef4\u590d\u5408\u6750\u6599\u7684\u6210\u578b\u5de5\u827a\u4e3b\u8981\u6709\u624b\u7cca\u53ca\u55b7\u5c04\u5de5\u827a\u3001\u70ed\u538b\u7f50\u6210\u578b\u3001\u6a21\u538b\u6210\u578b\u3001\u7f20\u7ed5\u3001\u62c9\u6324\u3001RTM\u5de5\u827a\u7b49\u3002<\/p>\n<p><strong>\uff081\uff09 \u624b\u7cca\u53ca\u55b7\u5c04\u5de5\u827a<\/strong><\/p>\n<p>\u624b\u7cca\u548c\u55b7\u5c04\u5de5\u827a\u9002\u5408\u6210\u578b\u5927\u578b\u3001\u590d\u6742\u6784\u4ef6\uff0c\u6210\u672c\u4f4e\u5ec9\uff0c\u5de5\u827a\u64cd\u4f5c\u7b80\u5355\uff0c\u5bf9\u64cd\u4f5c\u4eba\u5458\u8981\u6c42\u8f83\u4f4e\u3002\u5176\u7f3a\u70b9\u662f\u751f\u4ea7\u6548\u7387\u8f83\u4f4e\uff0c\u4ea7\u54c1\u8d28\u91cf\u53d7\u4eba\u4e3a\u56e0\u7d20\u5f71\u54cd\u8f83\u5927\u3002<\/p>\n<p><strong>\uff082\uff09 \u70ed\u538b\u7f50\u6210\u578b\u5de5\u827a<\/strong><br \/>\n<img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-62666\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/5-23.jpg\" alt=\"\" width=\"400\" height=\"140\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/5-23.jpg 400w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/5-23-300x105.jpg 300w\" sizes=\"(max-width: 400px) 100vw, 400px\" \/><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-62667\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/6-13.jpg\" alt=\"\" width=\"400\" height=\"172\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/6-13.jpg 400w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/6-13-300x129.jpg 300w\" sizes=\"(max-width: 400px) 100vw, 400px\" \/><br \/>\n\u70ed\u538b\u7f50\u6210\u578b\u5de5\u827a\u9002\u5408\u6210\u578b\u5927\u578b\u590d\u6742\u6784\u4ef6\uff0c\u9002\u5408\u6210\u578b\u9ad8\u7ea4\u7ef4\u4f53\u79ef\u5206\u6570\u7684\u590d\u5408\u6750\u6599\uff0c\u5176\u7f3a\u70b9\u4e3a\u8bbe\u5907\u6210\u672c\u9ad8\uff0c\u751f\u4ea7\u6548\u7387\u4f4e\u3002<\/p>\n<p><strong>\uff083\uff09 \u6a21\u538b\u6210\u578b\u5de5\u827a<\/strong><br \/>\n<img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-62668\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/7-12.jpg\" alt=\"\" width=\"400\" height=\"172\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/7-12.jpg 400w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/7-12-300x129.jpg 300w\" sizes=\"(max-width: 400px) 100vw, 400px\" \/><br \/>\n\u6a21\u538b\u6210\u578b\u9002\u5408\u6210\u578b\u5c0f\u578b\u590d\u6742\u6784\u4ef6\uff0c\u9002\u5408\u4e8e\u6210\u578b\u9ad8\u7ea4\u7ef4\u4f53\u79ef\u5206\u6570\u7684\u590d\u5408\u6750\u6599\uff0c\u5236\u54c1\u7684\u7cbe\u5ea6\u8f83\u9ad8\uff0c\u7f3a\u70b9\u5c31\u662f\u6210\u672c\u8f83\u9ad8\u3002<\/p>\n<p><strong>\uff084\uff09 \u7f20\u7ed5\u6210\u578b\u5de5\u827a<\/strong><\/p>\n<p>\u7f20\u7ed5\u5de5\u827a\u9002\u5408\u4e8e\u622a\u9762\u4e3a\u56de\u8f6c\u4f53\u7684\u590d\u5408\u6750\u6599\u4ea7\u54c1\u7684\u5236\u9020\uff0c\u4ea7\u54c1\u751f\u4ea7\u81ea\u52a8\u5316\u7a0b\u5ea6 \u9ad8\uff0c\u8d28\u91cf\u53ef\u63a7\u6027\u597d\uff0c\u5236\u5907\u5927\u578b\u6784\u4ef6\u9700\u8981\u5927\u578b\u7f20\u7ed5\u8bbe\u5907\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-62669\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/8-8.jpg\" alt=\"\" width=\"400\" height=\"229\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/8-8.jpg 400w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/8-8-300x172.jpg 300w\" sizes=\"(max-width: 400px) 100vw, 400px\" \/><br \/>\n<strong>\uff085\uff09 \u62c9\u6324\u6210\u578b\u5de5\u827a<\/strong><br \/>\n<img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-62670\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/9-4.jpg\" alt=\"\" width=\"400\" height=\"193\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/9-4.jpg 400w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/9-4-300x145.jpg 300w\" sizes=\"(max-width: 400px) 100vw, 400px\" \/><\/p>\n<p>\u62c9\u6324\u5de5\u827a\u9002\u5408\u5236\u5907\u7b49\u622a\u9762\u590d\u5408\u6750\u6599\u6784\u4ef6\uff0c\u751f\u4ea7\u6548\u7387\u9ad8\u3002<\/p>\n<p><strong>\uff086\uff09 RTM\u6210\u578b\u5de5\u827a<\/strong><\/p>\n<p>RTM\u5de5\u827a\u662f\u5c06\u9884\u5148\u9884\u5148\u6839\u636e\u8bbe\u8ba1\u94fa\u5c42\u7ed3\u6784\u7684\u589e\u5f3a\u6750\u6599\u9884\u6210\u578b\u4f53\u94fa\u653e\u5728\u6a21\u8154\u4e2d\uff0c\u901a\u8fc7\u4e00\u4e2a\u6216\u51e0\u4e2a\u6ce8\u5c04\u53e3\u5c06\u6811\u8102\u6ce8\u5165\u6a21\u8154\uff0c\u4f9d\u9760\u5e26\u538b\u6811\u8102\u7684\u6d41\u52a8\u6d78\u6da6\u7ea4\u7ef4\uff0c\u5e76\u6392\u9664\u6a21\u8154\u4e2d\u7684\u6c14\u4f53\uff0c\u56fa\u5316\u5f00\u6a21\uff0c\u6210\u578b\u5236\u54c1\u3002RTM\u5de5\u827a\u5177\u6709\u5c3a\u5bf8\u7a33\u5b9a\u6027\u597d\uff0c\u6210\u578b\u5468\u671f\u77ed\uff0c\u5236\u54c1\u8868\u9762\u5149\u6d01\u5ea6\u9ad8\u7b49\u7279\u5b9a\uff0c\u4f46\u7531\u4e8e\u6210\u578b\u91c7\u7528\u53cc\u7247\u6a21\u5177\uff0c\u6a21\u5177\u6210\u672c\u8f83\u9ad8\u3002<\/p>\n<p><span style=\"color: #0000ff;\"><strong>\u4e09\u3001 \u4ea7\u4e1a\u5e94\u7528<\/strong><\/span><\/p>\n<p>\u7531\u4e8e\u78b3\u7ea4\u7ef4\u590d\u5408\u6750\u6599\u5177\u6709\u9ad8\u6bd4\u5f3a\u5ea6\u548c\u6bd4\u6a21\u91cf\u3001\u5bc6\u5ea6\u5c0f\u3001\u53ef\u8bbe\u8ba1\u6027\u5f3a\u3001\u6613\u4e8e\u6574\u5f62\u7b49\u4f18\u70b9\uff0c\u968f\u7740\u9010\u6e10\u4ea7\u4e1a\u5316\uff0c\u5176\u88ab\u5e7f\u6cdb\u5e94\u7528\u4e8e\u822a\u7a7a\u822a\u5929\u3001\u6c7d\u8f66\u884c\u4e1a\u3001\u4f53\u80b2\u7528\u54c1\u3001\u6c11\u7528\u5176\u4ed6\u884c\u4e1a\u7b49\u9886\u57df\uff0c\u5df2\u7ecf\u6210\u4e3a\u4e86\u65b0\u4e00\u4ee3\u53ef\u5e94\u7528\u6750\u6599\u3002<\/p>\n<p><strong>1\u3001\u822a\u7a7a\u822a\u5929\u9886\u57df<\/strong><\/p>\n<p>\u78b3\u7ea4\u7ef4\u590d\u5408\u6750\u6599\u5728\u822a\u7a7a\u9886\u57df\u5f97\u5230\u4e86\u5927\u91cf\u5e94\u7528\u3002\u7f8e\u56fd\u6218\u673a\u8d85\u7ea7\u201c\u5927\u9ec4\u8702\u201d(F\/A-18E\/F)CFRP\u7528\u91cf\u7ea6\u4e3a19\uff05\uff0c\u6cd5\u56fd\u6218\u673a\u201c\u9635\u98ce\u201d\u7528\u91cf\u7ea6\u4e3a24\uff05\uff0c\u82f1\u56fd\u6218\u673a\u201c\u53f0\u98ce\u201d(EP2000)\u7528\u91cf\u7ea6\u4e3a40\uff05\u3002\u76f4\u5347\u98de\u673a\u4e5f\u5927\u91cf\u91c7\u7528CFRP\u3002\u4f8b\u5982\uff0c\u7531\u54c8\u5c14\u6ee8\u98de\u673a\u5236\u9020\u5382\u751f\u4ea7\u7684\u76f4-9\u578b\u76f4\u5347\u98de\u673a\uff0c\u6b66\u88c5\u4e86\u9a7b\u6e2f\u90e8\u961f\u548c\u53c2\u52a0\u4e862007\u5e74\u4e0a\u6d77\u5408\u4f5c\u7ec4\u7ec7\u5728\u4fc4\u7f57\u65af\u7684\u53cd\u6050\u519b\u6f14\uff0c\u662f\u6211\u56fd\u5148\u8fdb\u7684\u76f4\u5347\u98de\u673a\uff0c\u8be5\u673a\u590d\u5408\u6750\u6599\u7528\u91cf\u5df2\u5360\u523060\uff05\u5de6\u53f3\uff0c\u4e3b\u8981\u662fCFRP\u3002\u6b64\u5916\uff0c\u65e5\u672c\u751f\u4ea7\u7684\u201cOH-1\u5fcd\u8005\u201d\u76f4\u5347\u98de\u673a\uff0c\u673a\u8eab\u768440\uff05\u662f\u7528CFRP\uff0c\u6868\u53f6\u7b49\u4e5f\u7528CFRP\u5236\u9020\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-62672\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/12-4.jpg\" alt=\"\" width=\"400\" height=\"266\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/12-4.jpg 400w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/12-4-300x200.jpg 300w\" sizes=\"(max-width: 400px) 100vw, 400px\" \/><br \/>\nCFRP\u5728\u7a7a\u5ba2A380\u548c\u6ce2\u97f3787\u4e0a\u7684\u7528\u91cf\u5df2\u5360\u5230\u7ed3\u6784\u603b\u8d28\u91cf\u768450\uff05\uff0c\u79f0\u4e4b\u4e3a\u590d\u5408\u6750\u6599\u98de\u673a\u90fd\u4e0d\u4e3a\u8fc7\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-62673\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/11-1.jpg\" alt=\"\" width=\"400\" height=\"175\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/11-1.jpg 400w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/11-1-300x131.jpg 300w\" sizes=\"(max-width: 400px) 100vw, 400px\" \/><\/p>\n<p><strong>2\u3001\u6c7d\u8f66\u884c\u4e1a<\/strong><\/p>\n<p>\u968f\u7740\u4eba\u4eec\u5bf9\u751f\u6001\u73af\u4fdd\u7684\u91cd\u89c6\uff0c\u6c7d\u8f66\u7684\u8f7b\u91cf\u5316\u663e\u5f97\u8d8a\u6765\u8d8a\u91cd\u8981\uff0c\u8fd9\u66f4\u52a0\u5feb\u4e86\u78b3\u7ea4\u7ef4\u590d\u5408\u6750\u6599\u5728\u6c7d\u8f66\u4e2d\u7684\u4f7f\u7528\u3002 \u76ee\u524d\u78b3\u7ea4\u7ef4\u4e3b\u8981\u5e94\u7528\u5728\u5c0f\u6279\u91cf\u8f66\u578b\u3001\u9ad8\u7ea7\u8f7f\u8f66\u548cF1\u8d5b\u4e8b\u4e0a\u7684\u8f66\u4f53\u90e8\u5206\u3001\u53d1\u52a8\u673a\u90e8\u5206\u3001\u4f20\u52a8\u90e8\u5206\u3001\u5e95\u76d8\u7cfb\u7edf\u7b49\u3002\u5982\u6cd5\u62c9\u5229F430\u88c5\u5907\u7684\u5236\u52a8\u76d8\u3001\u9a6c\u81ea\u8fbeRX-8\u4f20\u52a8\u8f74\u3001\u4e30\u75301\/X\u6df7\u5408\u52a8\u529b\u8f66\u8f66\u8eab\u9aa8\u67b6\u3001\u5965\u8feaR8 Spyder\u8dd1\u8f66\u7684\u8f66\u9876\u3001\u884c\u674e\u7bb1\u7684\u4e24\u8fb9\u53ca\u9876\u90e8\uff0c\u5b9d\u9a6cM6\u578b\u7684\u9876\u84ec\u7b49\u90fd\u4e0d\u540c\u7a0b\u5ea6\u5730\u91c7\u7528\u4e86\u78b3\u7ea4\u7ef4\u590d\u5408\u6750\u6599\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-62674\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/13.jpg\" alt=\"\" width=\"400\" height=\"205\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/13.jpg 400w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/13-300x154.jpg 300w\" sizes=\"(max-width: 400px) 100vw, 400px\" \/><br \/>\n\u6700\u8fd1\u63a8\u51fa\u7684\u5b9d\u9a6ci8\u8dd1\u8f66\uff0c\u91c7\u7528\u5168\u65b0LC 500h\u7684\u78b3\u7ea4\u7ef4\u8f66\u9876\u3001\u78b3\u7ea4\u7ef4\u9aa8\u67b6\u7684\u94dd\u5408\u91d1\u8f66\u95e8\uff0c\u4ee5\u53ca\u5173\u952e\u90e8\u4f4d\u7684\u5927\u91cf\u8f7b\u8d28\u9ad8\u5f3a\u5ea6\u94a2\u6750\uff0c\u4f7f\u5f97\u5168\u65b0\u96f7\u514b\u8428\u65afLC\u7684\u8f66\u8eab\u6297\u626d\u521a\u6027\u751a\u81f3\u8d85\u8d8a\u4f20\u5947\u8dd1\u8f66LFA\uff0c\u4e3a\u5168\u65b0LC 500h\u5e26\u6765\u66f4\u4e3a\u7edf\u4e00\u3001\u7d27\u81f4\u7684\u64cd\u63a7\u8868\u73b0\u548c\u51cc\u5389\u7684\u8f6c\u5411\u54cd\u5e94\u3002<\/p>\n<p><strong>3\u3001\u4f53\u80b2\u5668\u6750<\/strong><\/p>\n<p>\u7531\u4e8e\u78b3\u7ea4\u7ef4\u590d\u5408\u6750\u6599\u9ad8\u5f3a\u9ad8\u6a21\u3001\u8d28\u91cf\u8f7b\u3001\u75b2\u52b3\u5f3a\u5ea6\u5927\u3001\u70ed\u81a8\u80c0\u7cfb\u6570\u5c0f\u3001\u7834\u635f\u5b89\u5168\u6027\u80fd\u597d\uff0c\u5176\u7528\u5728\u50cf\u6491\u6746\u3001\u9ad8\u5c14\u592b\u7403\u6746\u3001\u81ea\u884c\u8f66\u3001\u6ed1\u96ea\u677f\u3001\u76ae\u5212\u8247\u7b49\u9760\u4eba\u529b\u6765\u4f7f\u5176\u8fd0\u52a8\u7684\u4f53\u80b2\u5668\u6750\uff0c\u53ef\u4ee5\u5927\u5927\u63d0\u9ad8\u4f53\u80b2\u7ade\u6280\u7684\u6c34\u51c6\u3002<\/p>\n<p>\u78b3\u7ea4\u7ef4\u6491\u7aff\u53ef\u4ee5\u4fdd\u8bc1\u6491\u7aff\u65e2\u67d4\u97e7\u7ed3\u5b9e\u53c8\u4e0d\u4f1a\u65ad\u88c2\u6216\u626d\u7ed3\uff0c\u5b83\u53ef\u5c06\u8fd0\u52a8\u5458\u6301\u7aff\u5feb\u901f\u52a9\u8dd1\u7684\u52a8\u80fd\u90e8\u5206\u8f6c\u53d8\u6210\u6491\u7aff\u7684\u5f39\u6027\u53d8\u5f62\u80fd\uff0c\u5f53\u6491\u7aff\u88ab\u538b\u5f2f\u5230\u6700\u5927\u5f27\u5ea6\u540e\uff0c\u8fd9\u90e8\u5206\u5f39\u6027\u53d8\u5f62\u80fd\u518d\u91ca\u653e\u51fa\u6765\uff0c\u8f6c\u53d8\u6210\u8fd0\u52a8\u5458\u7684\u52bf\u80fd\uff0c\u5e2e\u52a9\u8fd0\u52a8\u5458\u817e\u7a7a\u8dc3\u8d77\uff0c\u98de\u8d8a\u6a2a\u6746\u3002\u968f\u7740\u73b0\u4ee3\u793e\u4f1a\u7684\u5feb\u901f\u53d1\u5c55\uff0c\u81ea\u884c\u8f66\u4e0d\u4ec5\u662f\u4ea4\u901a\u548c\u8fd0\u8f93\u5de5\u5177\uff0c\u8fd8\u5177\u6709\u5065\u8eab\u3001\u65c5\u6e38\u3001\u7ade\u8d5b\u7b49\u591a\u79cd\u529f\u80fd\u3002\u9ad8\u6863\u81ea\u884c\u8f66\u7684\u8f66\u6784\u67b6\u3001\u524d\u53c9\u90e8\u4ef6\u3001\u8f66\u8f6e\u3001\u66f2\u8f74\u53ca\u5ea7\u4f4d\u652f\u67b6\u7b49\u5747\u4f7f\u7528\u78b3\u7ea4\u7ef4\u590d\u5408\u6750\u6599\u5236\u6210\uff0c\u4e0d\u4ec5\u4f7f\u81ea\u884c\u8f66\u5916\u89c2\u66f4\u5177\u7f8e\u611f\uff0c\u540c\u65f6\u4e5f\u8d4b\u4e88\u4e86\u8f66\u4f53\u826f\u597d\u7684\u521a\u6027\u548c\u51cf\u9707\u6027\u80fd\u3002\u8f66\u4f53\u91cd\u91cf\u8fdb\u4e00\u6b65\u4e0b\u964d\uff0c\u9a91\u4e58\u8212\u9002\u6027\u66f4\u597d\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-62675\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/14.jpg\" alt=\"\" width=\"400\" height=\"223\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/14.jpg 400w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/14-300x167.jpg 300w\" sizes=\"(max-width: 400px) 100vw, 400px\" \/><\/p>\n<p>\u78b3\u7ea4\u7ef4\u590d\u5408\u6750\u6599\u9664\u4e86\u5e94\u7528\u5728\u4ee5\u4e0a\u51e0\u4e2a\u4e3b\u8981\u9886\u57df\u5916\uff0c\u8fd8\u6709\u5f88\u591a\u884c\u4e1a\u4f7f\u7528\u4e86\u78b3\u7ea4\u7ef4\u590d\u5408\u6750\u6599\uff0c\u50cf\u65e0\u4eba\u673a\u3001\u8239\u8236\u3001\u5bb6\u7535\u7b49\u7b49\uff0c\u7531\u4e8e\u7bc7\u5e45\u6709\u9650\uff0c\u5c0f\u7f16\u5c31\u4e0d\u518d\u4e00\u4e00\u5217\u4e3e\u4e86\u3002<\/p>\n<p><span style=\"color: #0000ff;\"><strong>\u56db\u3001 \u603b\u7ed3\u4e0e\u5c55\u671b<\/strong><\/span><\/p>\n<p>\u968f\u7740\u79d1\u6280\u7684\u53d1\u5c55\uff0c\u78b3\u7ea4\u7ef4\u590d\u5408\u6750\u6599\u5df2\u7ecf\u5728\u56fd\u5185\u5f88\u591a\u884c\u4e1a\u5f97\u5230\u4e86\u5e94\u7528\uff0c\u4f46\u7531\u4e8e\u78b3\u7ea4\u7ef4\u6280\u672f\u4e0d\u6210\u719f\uff0c\u5176\u751f\u4ea7\u6210\u672c\u8f83\u9ad8\uff0c\u5f88\u96be\u5f97\u5230\u5927\u89c4\u6a21\u4f7f\u7528\u30022016\u5e742\u670815\u65e5\uff0c\u4e2d\u56fd\u7ec8\u4e8e\u7a81\u7834\u65e5\u672c\u7ba1\u5236\u5c01\u9501\u7814\u5236\u51fa\u9ad8\u6027\u80fd\u78b3\u7ea4\u7ef4\u3002\u56fd\u5185\u7684\u78b3\u7ea4\u7ef4\u590d\u5408\u6750\u6599\u4e3b\u8981\u96c6\u4e2d\u5728\u5927\u578b\u56fd\u6709\u4f01\u4e1a\uff0c\u78b3\u7ea4\u7ef4\u590d\u5408\u6750\u6599\u7684\u771f\u6b63\u666e\u53ca\u8fd8\u9700\u8981\u9760\u5927\u91cf\u6c11\u4f01\u7684\u6280\u672f\u7a81\u7834\u6765\u8fdb\u884c\u63a8\u52a8\uff0c\u8fdb\u884c\u4f4e\u6210\u672c\u5316\u751f\u4ea7\uff0c\u771f\u6b63\u505a\u5230\u78b3\u7ea4\u7ef4\u590d\u5408\u6750\u6599\u5e7f\u6cdb\u5e94\u7528\u3002<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u7f16\u8f91\u90e8\u5b66\u672f\u5e72\u8d27\u7ec4\u6a0a\u8d85\u4f9b\u7a3f\uff0c\u6750\u6599\u725b\u7f16\u8f91\u6574\u7406\u3002<\/p>\n<p>\u6750\u6599\u4eba\u7f51\u4e13\u6ce8\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u53ca\u884c\u4e1a\u8fdb\u5c55\uff0c\u8fd9\u91cc\u6c47\u96c6\u4e86\u5404\u5927\u9ad8\u6821\u7855\u535a\u751f\u3001\u4e00\u7ebf\u79d1\u7814\u4eba\u5458\u4ee5\u53ca\u884c\u4e1a\u4ece\u4e1a\u8005\uff0c\u5982\u679c\u60a8\u5bf9\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u8fdb\u5c55\uff0c\u89e3\u8bfb\u9ad8\u6c34\u5e73\u6587\u7ae0\u6216\u662f\u8bc4\u8ff0\u884c\u4e1a\u6709\u5174\u8da3\uff0c<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\" target=\"_blank\">\u70b9\u6211\u52a0\u5165\u7f16\u8f91\u90e8<\/a>\u3002<\/p>\n<p>\u6750\u6599\u4eba\u7f51\u5411\u5404\u5927\u56e2\u961f\u8bda\u5fc3\u7ea6\u7a3f\uff0c\u8bfe\u9898\u7ec4\u6700\u65b0\u6210\u679c\u3001\u65b9\u5411\u603b\u7ed3\u3001\u56e2\u961f\u8bbf\u8c08\u3001\u5b9e\u9a8c\u6280\u80fd\u7b49\u7686\u53ef\u6295\u7a3f\uff0c\u4f18\u79c0\u7a3f\u4ef6\u4e00\u7ecf\u5f55\u7528\uff0c\u6211\u4eec\u4f1a\u5949\u4e0a\u7a3f\u916c\uff0c\u8bf7\u8054\u7cfb\uff1a\u90ae\u7bb1tougao@cailiaoren.com \u6216 QQ\uff1a97482208\u3002<\/p>\n<p>\u4eea\u5668\u8bbe\u5907\u3001\u8bd5\u5242\u8017\u6750\u3001\u6750\u6599\u6d4b\u8bd5\u3001\u6570\u636e\u5206\u6790\uff0c\u627e<a href=\"http:\/\/mai.cailiaoren.com\/\" target=\"_blank\">\u6750\u6599\u4eba<\/a>\u3001\u4e0a<a href=\"http:\/\/www.ceshigu.com\/\" target=\"_blank\">\u6d4b\u8bd5\u8c37<\/a>\uff01<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u4e00\u3001 \u7b80\u4ecb \u78b3\u7ea4\u7ef4\u662f\u7ea4\u7ef4\u72b6\u7684\u78b3\u7d20\u6750\u6599\uff0c\u542b\u78b3\u91cf\u572890%\u4ee5\u4e0a\uff0c\u5b83\u662f\u5229\u7528\u5404\u79cd\u6709\u673a\u7ea4\u7ef4\u5728\u60f0\u6027\u6c14\u4f53\u4e2d\uff0c\u9ad8\u6e29\u72b6\u6001\u4e0b\u78b3\u5316\u800c\u5236\u5f97\u7684\u3002\u78b3\u7ea4\u7ef4\u5177\u6709\u5341\u5206\u4f18\u5f02\u7684\u529b\u5b66\u6027\u80fd\uff0c\u662f\u76ee\u524d\u5df2\u5927\u91cf\u751f&#8230;<\/p>\n","protected":false},"author":842,"featured_media":62662,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[4],"tags":[43,76],"class_list":["post-62661","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-ganhuo","tag-composite","tag-carbon"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/62661"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/842"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=62661"}],"version-history":[{"count":12,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/62661\/revisions"}],"predecessor-version":[{"id":63111,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/62661\/revisions\/63111"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/62662"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=62661"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=62661"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=62661"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}