{"id":63201,"date":"2017-01-31T06:30:31","date_gmt":"2017-01-30T22:30:31","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=63201"},"modified":"2017-02-06T12:31:09","modified_gmt":"2017-02-06T04:31:09","slug":"%e5%ad%a6%e6%9c%af%e5%b9%b2%e8%b4%a7%e4%b8%a8%e5%b8%b8%e8%a7%81%e4%be%b5%e8%9a%80%e5%89%82%e5%8f%8a%e5%85%b6%e9%80%82%e7%94%a8%e7%9a%84%e9%87%91%e7%9b%b8%e7%bb%84%e7%bb%87","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=63201","title":{"rendered":"\u5b66\u672f\u5e72\u8d27\u4e28\u5e38\u89c1\u4fb5\u8680\u5242\u53ca\u5176\u9002\u7528\u7684\u91d1\u76f8\u7ec4\u7ec7"},"content":{"rendered":"<p>\u5728\u4e0e\u91d1\u5c5e\u6709\u5173\u7684\u5b9e\u9a8c\u8fc7\u7a0b\u4e2d\uff0c\u5f80\u5f80\u4e0d\u53ef\u907f\u514d\u7684\u8981\u7528\u5230\u91d1\u76f8\u8bd5\u6837\u5236\u5907\u6280\u672f\uff0c\u800c\u5176\u4e2d\u6700\u4e3a\u5173\u952e\u7684\u662f\u9488\u5bf9\u4e00\u5b9a\u7684\u6750\u6599\u9009\u62e9\u5408\u9002\u7684\u4fb5\u8680\u5242\u53ca\u4fb5\u8680\u65b9\u6cd5\uff0c\u53ea\u6709\u8fd9\u6837\u624d\u80fd\u5236\u597d\u6211\u4eec\u9700\u8981\u7684\u91d1\u76f8\u8bd5\u6837\u3002\u8fd9\u91cc\uff0c\u6211\u4eec\u5c31\u5c06\u5e38\u89c1\u7684\u4fb5\u8680\u5242\u53ca\u5176\u9002\u7528\u5bf9\u8c61\u4e0e\u65b9\u6cd5\u7b80\u5355\u7f57\u5217\u5982\u4e0b\u3002<\/p>\n<table width=\"707\">\n<tbody>\n<tr>\n<td width=\"45\">\u5e8f\u53f7<\/td>\n<td width=\"198\">\u6210\u5206<\/td>\n<td width=\"171\">\u9002\u7528\u5bf9\u8c61<\/td>\n<td width=\"142\">\u8150\u8680\u65b9\u6cd5<\/td>\n<td width=\"151\">\u5907\u6ce8<\/td>\n<\/tr>\n<tr>\n<td width=\"45\">1<\/td>\n<td width=\"198\">1:1(\u5bb9\u79ef\u6bd4\u5de5\u4e1a\u76d0\u9178\u6c34\u6eb6\u6db2)<\/td>\n<td width=\"171\">\u5927\u591a\u6570\u94a2\u79cd<\/td>\n<td width=\"142\"><\/td>\n<td rowspan=\"2\" width=\"151\">\u9178\u8680\u540e\u9632\u9508\u65b9\u6cd5:<\/p>\n<p>a.\u4e2d\u548c\u6cd5:\u752810%\u6c28\u6c34\u6eb6\u6db2\u6d78\u6ce1\u540e\u518d\u4ee5\u70ed\u6c34\u51b2\u6d17\u3002<\/p>\n<p>b.\u949d\u5316\u6cd5:\u6d78\u5165\u6d53\u785d\u91785\u79d2\u518d\u7528\u70ed\u6c34\u51b2\u6d17\u3002<\/p>\n<p>c.\u6d82\u5c42\u4fdd\u62a4\u6cd5:\u6d82\u6e05\u6f06\u548c\u5851<\/td>\n<\/tr>\n<tr>\n<td width=\"45\">2<\/td>\n<td width=\"198\">\u76d0\u917810\u4efd\uff0c\u785d\u91781\u4efd\uff0c\u6c3410\u4efd\uff08\u5bb9\u79ef\u6bd4\uff09<\/td>\n<td width=\"171\">\u5965\u6c0f\u4f53<\/p>\n<p>\u4e0d\u9508\u94a2<\/p>\n<p>\u8010\u70ed\u94a2<\/td>\n<td width=\"142\">60-70\u2103\u70ed\u8680\u65f6\u95f4:\u00a05-25min<\/td>\n<\/tr>\n<tr>\n<td width=\"45\">3<\/td>\n<td width=\"198\">\u76d0\u917838\u4efd\uff0c\u786b\u917812\u4efd\uff0c\u6c3450\u4efd\uff08\u5bb9\u79ef\u6bd4\uff09<\/td>\n<td width=\"171\">\u78b3\u7d20\u94a2<\/p>\n<p>\u5408\u91d1\u94a2<\/p>\n<p>\u9ad8\u901f\u5de5\u5177\u94a2<\/td>\n<td width=\"142\">60-80\u2103\u70ed\u8680\u65f6\u95f4:\u00a015~25min<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">4<\/td>\n<td width=\"198\">\u76d0\u9178500mL,\u786b\u917835mL\uff0c\u94dc150g<\/td>\n<td width=\"171\">\u5927\u591a\u6570\u94a2\u79cd<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/p>\n<p>\u5728\u6d78\u8680\u8fc7\u7a0b\u4e2d,\u7528\u00a0\u00a0\u6bdb\u5237\u4e0d\u65ad\u64e6\u62ed\u8bd5\u6837\u8868\u9762,\u00a0\u53bb\u9664\u8868\u9762\u6c89\u6dc0\u7269<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">5<\/td>\n<td width=\"198\">\u4e09\u6c2f\u5316\u94c1200g\uff0c\u785d\u9178300mL\uff0c\u6c34100mL<\/td>\n<td width=\"171\">\u5927\u591a\u6570\u94a2\u79cd<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680\u6216\u64e6\u62ed1~5min<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">6<\/td>\n<td width=\"198\">\u76d0\u917830mL\uff0c\u4e09\u6c2f\u5316\u94c150g\uff0c\u6c3470 mL<\/td>\n<td width=\"171\">\u5927\u591a\u6570\u94a2\u79cd<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">7<\/td>\n<td width=\"198\">10%~40%\u785d\u9178\u6c34\u6eb6\u6db2\u00a0(\u5bb9\u79ef\u6bd4)<\/td>\n<td width=\"171\">\u78b3\u7d20\u94a2<\/p>\n<p>\u5408\u91d1\u94a2<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u868025%\u785d\u9178\u6c34\u6eb6\u6db2\u4e3a\u901a\u7528\u6d78\u8680\u5242<\/td>\n<td rowspan=\"2\" width=\"151\">a.\u53ef\u7528\u4e8e\u7403\u58a8\u94f8\u94c1\u7684\u4f4e\u500d\u7ec4\u7ec7\u663e<\/p>\n<p>\u793a\u3002<\/p>\n<p>b.\u9ad8\u6d53\u5ea6\u9002\u7528\u4e8e\u4e0d\u4fbf\u4f5c\u52a0\u70ed\u7684\u94a2\u952d\u622a\u9762\u7b49\u5927\u8bd5\u6837\u3002<\/td>\n<\/tr>\n<tr>\n<td width=\"45\">8<\/td>\n<td width=\"198\">10%~20%\u8fc7\u786b\u9178\u94f5\u6c34\u6eb6\u6db2<\/td>\n<td width=\"171\">\u78b3\u7d20\u94a2<\/p>\n<p>\u5408\u91d1\u94a2<\/p>\n<p>\u663e\u793a\u6280\u6676\u53ca\u7c97\u6676\u7ec4\u7ec7<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680\u6216\u64e6\u62ed<\/td>\n<\/tr>\n<tr>\n<td width=\"45\">9<\/td>\n<td width=\"198\">\u4e09\u6c2f\u5316\u94c1\u9971\u548c\u6c34\u6eb6500ml<\/p>\n<p>\u785d\u9178\u00a0\u00a010ml<\/td>\n<td width=\"171\">\u78b3\u7d20\u94a2\u00a0\u5408\u91d1\u94a2<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">10<\/td>\n<td width=\"198\">\u785d\u9178\u00a01\u4efd\u00a0\u76d0\u9178\u00a03\u4efd<\/td>\n<td width=\"171\">\u4e0d\u9508\u94a2\u53ca<\/p>\n<p>\u9ad8\u94ec\u9ad8\u954d\u5408\u91d1\u94a2<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">11<\/td>\n<td width=\"198\">\u786b\u9178\u94dc\u6eb6\u6db2100mL\uff0c\u76d0\u9178500mL,\u6c34500mL<\/td>\n<td width=\"171\">\u5965\u6c0f\u4f53\u4e0d\u9508\u94a2<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680\u00a0\u00a0\u4e5f\u53ef\u4ee5\u52a0\u70ed\u4f7f\u7528<\/td>\n<td width=\"151\">\u901a\u7528\u6d78\u8680\u5242<\/td>\n<\/tr>\n<tr>\n<td width=\"45\">12<\/td>\n<td width=\"198\">\u785d\u917860mL,\u76d0\u9178200mL\uff0c\u6c2f\u5316\u9ad8\u94c150g\uff0c\u8fc7\u786b\u9178\u94f530g\uff0c\u6c3450mL<\/td>\n<td width=\"171\">\u7cbe\u5bc6\u5408\u91d1\u00a0\u9ad8\u6e29\u5408\u91d1<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">13<\/td>\n<td width=\"198\">\u5de5\u4e1a\u6c2f\u5316\u94dc\u94f512g\uff0c\u76d0\u91785mL\uff0c\u6c34100mL<\/td>\n<td width=\"171\">\u94a2\u7684\u7ed3\u6676\u7ec4\u7ec7<\/td>\n<td width=\"142\">\u6d78\u868030~60min<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">14<\/td>\n<td width=\"198\">\u785d\u917810mL\uff0c\u786b\u917810mL\uff0c\u6c3420mL<\/td>\n<td width=\"171\">\u663e\u793a\u94f8\u6001<\/p>\n<p>\u7ec4\u7ec7\u548c\u94f8\u94a2\u6676\u7c92\u5ea6<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">15<\/td>\n<td width=\"198\">\u76d0\u917850mL\uff0c\u785d\u917825mL\uff0c\u6c3425mL<\/td>\n<td width=\"171\">\u9ad8\u5408\u91d1\u94a2\u00a0\u00a0\u9ad8\u901f\u94a2<\/p>\n<p>\u94c1-\u94b4\u548c\u954d\u57fa\u9ad8\u6e29\u5408\u91d1<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/td>\n<td width=\"151\">\u7a00\u738b\u6c34\u6d78\u8680\u5242<\/td>\n<\/tr>\n<tr>\n<td width=\"45\">16<\/td>\n<td width=\"198\">\u91cd\u94ec\u9178\u94be\u00a0\u00a025g\uff0c\u76d0\u9178100mL\uff0c\u785d\u917810mL\uff0c\u6c34100mL<\/td>\n<td width=\"171\">\u94c1\u7d20\u4f53\u53ca<\/p>\n<p>\u5965\u6c0f\u4f53\u4e0d\u9508\u94a2<\/td>\n<td width=\"142\">60~70\u2103\u70ed\u8680\uff0c\u65f6\u95f4:30~60min<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">17<\/td>\n<td width=\"198\">Nital:\u785d\u91781~5mL\u9152\u7cbe100mL<\/td>\n<td width=\"171\">\u6dec\u706b\u9a6c\u6c0f\u4f53\u3001\u73e0\u5149\u4f53\u3001\u94f8\u94c1\u7b49<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<table width=\"707\">\n<tbody>\n<tr>\n<td width=\"45\">18<\/td>\n<td width=\"198\">Picral: \u82e6\u5473\u91784g, \u9152\u7cbe100mL<\/td>\n<td width=\"170\">\u73e0\u5149\u4f53\u3001\u9a6c\u6c0f\u4f53\u3001\u8d1d\u6c0f\u4f53\u3001\u6e17\u78b3\u4f53<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">19<\/td>\n<td width=\"198\">Vilella\u2019s: \u76d0\u91785mL, \u82e6\u5473\u91781g, \u82e6\u5473\u91781g<\/td>\n<td width=\"170\">\u56de\u706b\u9a6c\u6c0f\u4f53\u53ca\u5965\u6c0f\u4f53\u6676\u7c92<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">20<\/td>\n<td width=\"198\">\u76d0\u917810mL, \u785d\u91783mL, \u9152\u7cbe100mL<\/td>\n<td width=\"170\">\u9ad8\u901f\u94a2\u56de\u706b\u540e\u6676\u7c92\u3001\u6c2e\u5316\u5c42\u3001\u78b3\u6c2e\u5316\u5c42<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">21<\/td>\n<td width=\"198\">\u6c2f\u5316\u9ad8\u94c15g\u76d0\u917815mL<\/p>\n<p>\u6c34100mL<\/td>\n<td width=\"170\">\u7eaf\u94dc\u3001\u9ec4\u94dc\u53ca\u5176\u4ed6\u94dc\u5408\u91d1<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">22<\/td>\n<td width=\"198\">(NH<sub>4<\/sub>)<sub>2<\/sub>S<sub>2<\/sub>O<sub>3<\/sub>\u00a010g \u6c34100mL<\/td>\n<td width=\"170\">\u7eaf\u94dc\u3001\u9ec4\u94dc\u53ca\u5176\u4ed6\u94dc\u5408\u91d1<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">23<\/td>\n<td width=\"198\">\u6c22\u6c1f\u91781mL\u6c34200m\u00a0L<\/td>\n<td width=\"170\">\u94dd\u53ca\u94dd\u5408\u91d1<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">24<\/td>\n<td width=\"198\">\u6c22\u6c27\u5316\u94a01g \u6c34100mL<\/td>\n<td width=\"170\">\u94dd\u53ca\u94dd\u5408\u91d1<\/td>\n<td width=\"142\">\u4e0d\u8981\u6cbe\u67d3\u76ae\u80a4<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">25<\/td>\n<td width=\"198\">Keller\u2019s: \u00a0\u6c22\u6c1f\u91782mL<\/p>\n<p>\u76d0\u91783mL \u785d\u91785mL<\/p>\n<p>\u6c34190m\u00a0L<\/td>\n<td width=\"170\">\u94dd\u53ca\u94dd\u5408\u91d1<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">26<\/td>\n<td width=\"198\">Marble\u2019s: \u786b\u9178\u94dc5g<\/p>\n<p>\u76d0\u917850mL \u6c3450mL<\/td>\n<td width=\"170\">\u9ad8\u6e29\u5408\u91d1<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">27<\/td>\n<td width=\"198\">Murakami&#8217;s: \u8d64\u8840\u76d05g(10g)<\/p>\n<p>\u6c22\u6c27\u5316\u94a05g(10g)<\/p>\n<p>\u6c34100mL<\/td>\n<td width=\"170\">\u78b3\u5316\u949b\u9540\u5c42<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">228<\/td>\n<td width=\"198\">Kalling&#8217;s\u00a01: \u6c2f\u5316\u94dc2g<\/p>\n<p>\u76d0\u917840mL<\/p>\n<p>95%\u4e59\u918740~80mL<\/p>\n<p>\u6c3440mL<\/td>\n<td width=\"170\"><\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">29<\/td>\n<td width=\"198\">Kalling&#8217;s\u00a02: \u6c2f\u5316\u94dc2g<\/p>\n<p>\u76d0\u917840mL<\/p>\n<p>95%\u4e59\u918740~80mL<\/td>\n<td width=\"170\"><\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">30<\/td>\n<td width=\"198\">90~99ml\u7532\u9187\u6216\u9152\u7cbe+1~10ml\u785d\u9178<\/td>\n<td width=\"170\">\u9002\u7528\u4e8e\u94c1\uff0c\u78b3\u94a2\uff0c\u5408\u91d1\u94a2\u4ee5\u53ca\u94f8\u94c1\u7684\u5e38\u7528\u8150\u8680\u5242\uff0c\u663e\u793aa\u6676\u754c\u53ca\u7ec4\u7ec7\u3002<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">31<\/td>\n<td width=\"198\">100mL\u9152\u7cbe+4g\u82e6\u5473\u9178<\/td>\n<td width=\"170\">\u591a\u7528\u4e8e\u94c1\u7d20\u4f53\u548c\u78b3\u5316\u7269\u7ec4\u6210\u7684\u7ec4\u7ec7\u7ed3\u6784\uff0c\u4e0d\u80fd\u663e\u793a\u94c1\u7d20\u4f53\u6676\u754c<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">32<\/td>\n<td width=\"198\">\u9971\u548c\u82e6\u5473\u9178<\/p>\n<p>\u5c11\u91cf\u6da6\u6ed1\u5242<\/td>\n<td width=\"170\">\u591a\u7528\u4e8e\u663e\u793a\u521d\u751f\u5965\u6c0f\u4f53\u6676\u754c\uff0c\u975e\u5e38\u9002\u7528\u4e8e\u9a6c\u6c0f\u4f53\u548c\u8d1d\u6c0f\u4f53\u94a2<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">33<\/td>\n<td width=\"198\">150mL\u6c34\u00a0 50mL\u76d0\u9178<\/p>\n<p>25mL\u785d\u9178 1g\u6c2f\u5316\u94dc<\/td>\n<td width=\"170\">\u7528\u4e8e\u542b18\uff05\u954d\u7684\u9a6c\u6c0f\u4f53\u65f6\u6548\u94a2\uff0c\u9a6c\u6c0f\u4f53\u548c\u6c89\u6dc0\u786c\u5316\u4e0d\u9508\u94a2<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">34<\/td>\n<td width=\"198\">100mL\u6c34<\/p>\n<p>25g NaOH<\/p>\n<p>2g\u82e6\u5473\u9178<\/td>\n<td width=\"170\">\u7279\u522b\u9002\u7528\u4e8eMcQuaid-Ehn\u78b3\u5316\u8bd5\u6837\uff0cDarkens\u78b3\u5316\u7269\uff0c\u6eb6\u6db2\u8150\u86801~15\u5206\u949f\u6216\u7535\u89e3\u8150\u86806V\uff08DC\uff09,0.5A\/cm<sup>2<\/sup>,30~120\u79d2\u53ef\u4ee5\u663e\u793a\u9ad8\u78b3\u94a2\u5965\u6c0f\u4f53\u6676\u754c<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">35<\/td>\n<td width=\"198\">3\u4efd\u76d0\u9178+2\u4efd\u7518\u6cb9+1\u4efd\u785d\u9178<\/td>\n<td width=\"170\">\u9002\u7528\u4e8e\u5965\u6c0f\u4f53\u4e0d\u9508\u94a2\u3002\u663e\u793a\u6676\u7c92\u7ed3\u6784\uff0c\u548c\u78b3\u5316\u7269\u7684\u8f6e\u5ed3\uff0c\u73b0\u7528\u73b0\u914d\uff0c\u4e0d\u80fd\u50a8\u5b58\uff0c\u64e6\u62ed\u8bd5\u6837<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">36<\/td>\n<td width=\"198\">100mL\u9152\u7cbe+100mL\u76d0\u9178+5g\u6c2f\u5316\u94dc<\/td>\n<td width=\"170\">\u7528\u4e8e\u5965\u6c0f\u4f53\u548c\u53cc\u76f8\u4e0d\u9508\u94a2\uff0c\u94c1\u7d20\u4f53\u5bb9\u6613\u4fb5\u8680\uff0c\u78b3\u5316\u7269\u4e0d\u88ab\u4fb5\u8680\uff0c\u5965\u6c0f\u4f53\u88ab\u8f7b\u5ea6\u8150\u8680\uff0c\u5ba4\u6e29\u4e0b\u64e6\u62ed\u6216\u4fb5\u8680\uff0c\u53ef\u4ee5\u50a8\u5b58<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">37<\/td>\n<td width=\"198\">15mL\u76d0\u9178 10mL\u918b\u9178<\/p>\n<p>5mL\u785d\u9178\u00a0 2\u6ef4\u7518\u6cb9<\/td>\n<td width=\"170\">\u9002\u7528\u4e8e\u9ad8\u5408\u91d1\u4e0d\u9508\u94a2\uff0c\u5148\u7528\u73b0\u914d<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">38<\/td>\n<td width=\"198\">100mL\u6c34<\/p>\n<p>+K<sub>2<\/sub>Fe(CN)<sub>6<\/sub>+10gKOH\u6216NaOH<\/td>\n<td width=\"170\">\u591a\u9002\u7528\u4e8e\u94c1\u7d20\u4f53\u4e0d\u9508\u94a2\uff0c\u94c1\u7d20\u4f53\u53d1\u9ec4\u6216\u8005\u68d5\u9ec4\uff0c\u5965\u6c0f\u4f53\u4e0d\u88ab\u4fb5\u8680<\/td>\n<td width=\"142\">CN<sup>&#8211;<\/sup>\u6709\u5267\u6bd2\uff0c\u6ce8\u610f\u5b89\u5168<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">39<\/td>\n<td width=\"198\">100mL\u6c34+10g\u8349\u9178<\/td>\n<td width=\"170\">6 V \uff08DC\uff09\u7528\u4e8e\u4e0d\u9508\u94a2\u7535\u89e3\u8150\u8680\uff0c15~30\u79d2\u663e\u793a\u78b3\u5316\u7269\uff0c45~60\u79d2\u663e\u793a\u6676\u754c<\/td>\n<td width=\"142\">\u5ba4\u6e29\u6d78\u8680<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<tr>\n<td width=\"45\">40<\/td>\n<td width=\"198\">100mL\u6c34+20gNaOH<\/td>\n<td width=\"170\">\u7528\u4e8e\u9a6c\u6c0f\u4f53\uff0c\u6c89\u6dc0\u786c\u5316\u6210\u53cc\u76f8\u94a2\u4e2d\u94c1\u7d20\u4f53\u7684\u7740\u8272<\/td>\n<td width=\"142\">3~5 V\uff08DC\uff09\uff0c20\u2103\uff0c5\u79d2\uff0c\u663e\u793a\u94c1\u7d20\u4f53\u8f6e\u5ed3\u548c\u7740\u6df1\u68d5\u8910\u8272<\/td>\n<td width=\"151\"><\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u7f16\u8f91\u90e8\u5b66\u672f\u5e72\u8d27\u7ec4\u7267\u7f8a\u4eba\u4f9b\u7a3f\uff0c\u6750\u6599\u725b\u7f16\u8f91\u6574\u7406\u3002<\/p>\n<p>\u6750\u6599\u4eba\u7f51\u4e13\u6ce8\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u53ca\u884c\u4e1a\u8fdb\u5c55\uff0c\u8fd9\u91cc\u6c47\u96c6\u4e86\u5404\u5927\u9ad8\u6821\u7855\u535a\u751f\u3001\u4e00\u7ebf\u79d1\u7814\u4eba\u5458\u4ee5\u53ca\u884c\u4e1a\u4ece\u4e1a\u8005\uff0c\u5982\u679c\u60a8\u5bf9\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u8fdb\u5c55\uff0c\u89e3\u8bfb\u9ad8\u6c34\u5e73\u6587\u7ae0\u6216\u662f\u8bc4\u8ff0\u884c\u4e1a\u6709\u5174\u8da3\uff0c<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\" target=\"_blank\">\u70b9\u6211\u52a0\u5165\u7f16\u8f91\u90e8<\/a>\u3002<\/p>\n<p>\u6750\u6599\u4eba\u7f51\u5411\u5404\u5927\u56e2\u961f\u8bda\u5fc3\u7ea6\u7a3f\uff0c\u8bfe\u9898\u7ec4\u6700\u65b0\u6210\u679c\u3001\u65b9\u5411\u603b\u7ed3\u3001\u56e2\u961f\u8bbf\u8c08\u3001\u5b9e\u9a8c\u6280\u80fd\u7b49\u7686\u53ef\u6295\u7a3f\uff0c\u4f18\u79c0\u7a3f\u4ef6\u4e00\u7ecf\u5f55\u7528\uff0c\u6211\u4eec\u4f1a\u5949\u4e0a\u7a3f\u916c\uff0c\u8bf7\u8054\u7cfb\uff1a\u90ae\u7bb1tougao@cailiaoren.com \u6216 QQ\uff1a97482208\u3002<\/p>\n<p>\u4eea\u5668\u8bbe\u5907\u3001\u8bd5\u5242\u8017\u6750\u3001\u6750\u6599\u6d4b\u8bd5\u3001\u6570\u636e\u5206\u6790\u3001\u627e<a href=\"http:\/\/www.cailiaoren.com\/\" target=\"_blank\">\u6750\u6599\u4eba<\/a>\u3001\u4e0a<a href=\"http:\/\/www.ceshigu.com\/\" target=\"_blank\">\u6d4b\u8bd5\u8c37<\/a>\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u5728\u4e0e\u91d1\u5c5e\u6709\u5173\u7684\u5b9e\u9a8c\u8fc7\u7a0b\u4e2d\uff0c\u5f80\u5f80\u4e0d\u53ef\u907f\u514d\u7684\u8981\u7528\u5230\u91d1\u76f8\u8bd5\u6837\u5236\u5907\u6280\u672f\uff0c\u800c\u5176\u4e2d\u6700\u4e3a\u5173\u952e\u7684\u662f\u9488\u5bf9\u4e00\u5b9a\u7684\u6750\u6599\u9009\u62e9\u5408\u9002\u7684\u4fb5\u8680\u5242\u53ca\u4fb5\u8680\u65b9\u6cd5\uff0c\u53ea\u6709\u8fd9\u6837\u624d\u80fd\u5236\u597d\u6211\u4eec\u9700\u8981\u7684\u91d1\u76f8\u8bd5\u6837\u3002&#8230;<\/p>\n","protected":false},"author":579,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[4],"tags":[],"class_list":["post-63201","post","type-post","status-publish","format-standard","hentry","category-ganhuo"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/63201"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/579"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=63201"}],"version-history":[{"count":1,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/63201\/revisions"}],"predecessor-version":[{"id":63228,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/63201\/revisions\/63228"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=63201"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=63201"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=63201"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}