{"id":68013,"date":"2017-02-25T18:00:53","date_gmt":"2017-02-25T10:00:53","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=68013"},"modified":"2017-11-11T23:09:33","modified_gmt":"2017-11-11T15:09:33","slug":"%e5%ae%9e%e9%aa%8c%e6%8a%80%e8%83%bd%e4%b8%a8%e6%9e%81%e7%ae%80%e7%9a%84dsc%e5%8e%9f%e7%90%86%e4%b8%8e%e6%b5%8b%e8%af%95%e7%bb%8f%e5%85%b8%e9%97%ae%e7%ad%94%e5%85%a5%e9%97%a8","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=68013","title":{"rendered":"\u5b9e\u9a8c\u6280\u80fd\u4e28TG-DSC\u539f\u7406\u4e0e\u6d4b\u8bd5\u5165\u95e8\u7ecf\u5178\u95ee\u7b54"},"content":{"rendered":"<p><strong>\u8bf7\u8bb2\u4e00\u8bb2DSC\u57fa\u672c\u539f\u7406\u4e0e\u7ecf\u5178\u5e94\u7528\uff1f<\/strong><\/p>\n<p>\u5728\u7a0b\u5e8f\u6e29\u5ea6\uff08\u5347\uff0f\u964d\uff0f\u6052\u6e29\u53ca\u5176\u7ec4\u5408\uff09\u8fc7\u7a0b\u4e2d\uff0c\u6d4b\u91cf\u6837\u54c1\u4e0e\u53c2\u8003\u7269\u4e4b\u95f4\u7684\u70ed\u6d41\u5dee\uff0c\u4ee5\u8868\u5f81\u6240\u6709\u4e0e\u70ed\u6548\u5e94\u6709\u5173\u7684\u7269\u7406\u53d8\u5316\u548c\u5316\u5b66\u53d8\u5316\u3002<\/p>\n<p><strong>\u5178\u578b\u5e94\u7528\uff1a<\/strong><\/p>\n<table style=\"height: 164px;\" width=\"592\">\n<tbody>\n<tr>\n<td style=\"width: 288px;\">\u73bb\u7483\u5316\u8f6c\u53d8<\/td>\n<td style=\"width: 288px;\">\u76f8\u5bb9\u6027<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 288px;\">\u7194\u878d\u3001\u7ed3\u6676<\/td>\n<td style=\"width: 288px;\">\u70ed\u7a33\u5b9a\u6027\u3001\u6c27\u5316\u7a33\u5b9a\u6027<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 288px;\">\u7194\u878d\u70ed\u3001\u7ed3\u6676\u70ed<\/td>\n<td style=\"width: 288px;\">\u53cd\u5e94\u52a8\u529b\u5b66<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 288px;\">\u5171\u7194\u6e29\u5ea6\u3001\u7eaf\u5ea6<\/td>\n<td style=\"width: 288px;\">\u70ed\u529b\u5b66\u51fd\u6570<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 288px;\">\u7269\u8d28\u9274\u522b<\/td>\n<td style=\"width: 288px;\">\u6db2\u76f8\u3001\u56fa\u76f8\u6bd4\u4f8b<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 288px;\">\u591a\u6676\u578b<\/td>\n<td style=\"width: 288px;\">\u6bd4\u70ed<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p><strong>DSC\u4e0eDTA\u662f\u4ec0\u4e48\u5173\u7cfb\uff1f<\/strong><\/p>\n<p>DSC\u7684\u524d\u8eab\u662f\u5dee\u70ed\u5206\u6790DTA\uff0c\u6211\u7b80\u5355\u4ecb\u7ecd\u4e0b\u5de5\u4f5c\u539f\u7406\u7684\u533a\u522b<\/p>\n<p>DTA\u5462\uff0c\u53ea\u80fd\u6d4b\u8bd5\u25b3T\u4fe1\u53f7\uff0c\u65e0\u6cd5\u5efa\u7acb\u25b3H\u4e0e\u25b3T\u4e4b\u95f4\u7684\u8054\u7cfb<\/p>\n<p>\u800cDSC\u6d4b\u8bd5\u25b3T\u4fe1\u53f7\uff0c\u5e76\u5efa\u7acb\u25b3H\u4e0e\u25b3T\u4e4b\u95f4\u7684\u8054\u7cfb<\/p>\n<p><strong>DSC\u6d4b\u8bd5\u9700\u8981\u6ce8\u610f\u54ea\u4e9b\u6761\u4ef6\uff1f<\/strong><\/p>\n<p>\u4e3b\u8981\u6709\u5982\u4e0b\u51e0\u70b9\uff1a\u5347\u6e29\u901f\u7387\u3001\u6837\u54c1\u7528\u91cf\u3001\u5236\u6837\u65b9\u5f0f\u3001\u5b9e\u9a8c\u6c14\u6c1b\u3001\u5769\u57da\u7684\u9009\u53d6\u3001\u6837\u54c1\u6e29\u5ea6\u63a7\u5236\uff08STC\uff09\u3001DSC\u57fa\u7ebf\u3002<\/p>\n<p><strong>\u5347\u6e29\u901f\u7387\u6709\u54ea\u4e9b\u5f71\u54cd\uff0c\u6709\u6ca1\u6709\u6807\u51c6\u7684\u5347\u6e29\u901f\u7387\uff1f<\/strong><\/p>\n<table style=\"height: 90px;\" width=\"614\">\n<tbody>\n<tr style=\"height: 24px;\">\n<td style=\"width: 299px; height: 24px; text-align: center;\"><strong>\u5feb\u901f\u5347\u6e29<\/strong><\/td>\n<td style=\"width: 299px; height: 24px; text-align: center;\"><strong>\u6162\u901f\u5347\u6e29<\/strong><\/td>\n<\/tr>\n<tr style=\"height: 24px;\">\n<td style=\"width: 299px; height: 24px; text-align: center;\">\u4f7fDSC\u5cf0\u5f62\u53d8\u5927<\/td>\n<td style=\"width: 299px; height: 24px; text-align: center;\">\u6709\u5229\u4e8e\u76f8\u90bb\u5cf0\u6216\u76f8\u90bb\u5931\u91cd\u5e73\u53f0\u7684\u5206\u79bb<\/td>\n<\/tr>\n<tr style=\"height: 27px;\">\n<td style=\"width: 299px; height: 27px; text-align: center;\">\u7279\u5f81\u6e29\u5ea6\u5411\u9ad8\u6e29\u6f02\u79fb<\/td>\n<td style=\"width: 299px; height: 27px; text-align: center;\">DSC\/DTA\u5cf0\u5f62\u8f83\u5c0f<\/td>\n<\/tr>\n<tr style=\"height: 24px;\">\n<td style=\"width: 299px; height: 24px; text-align: center;\">\u76f8\u90bb\u5cf0\u6216\u5931\u91cd\u53f0\u9636\u7684\u5206\u79bb\u80fd\u529b\u4e0b\u964d<\/td>\n<td style=\"width: 299px; height: 24px; text-align: center;\">\u2014\u2014\u2014\u2014\u2014\u2014\u2014\u2014\u2014\u2014<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p><a href=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/02\/\u6e29\u5ea6\u7684\u5f71\u54cd-1.png\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-68031\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/02\/\u6e29\u5ea6\u7684\u5f71\u54cd-1.png\" alt=\"\" width=\"512\" height=\"384\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/02\/\u6e29\u5ea6\u7684\u5f71\u54cd-1.png 512w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/02\/\u6e29\u5ea6\u7684\u5f71\u54cd-1-300x225.png 300w\" sizes=\"(max-width: 512px) 100vw, 512px\" \/><\/a><\/p>\n<p>\u70ed\u5206\u6790\u9886\u57df\u5e38\u7528\u800c\u6807\u51c6\u7684\u5347\u6e29\u901f\u7387\u662f<strong><span style=\"text-decoration: underline;\">10K\/min<\/span><\/strong><\/p>\n<p>\u5229\u7528\u591a\u4e2a\u4e0d\u540c\u5347\u6e29\u901f\u7387\u4e0b\u5f97\u5230\u7684\u4e00\u7cfb\u5217\u6d4b\u8bd5\u7ed3\u679c\uff0c\u53ef\u8fdb\u884c\u52a8\u529b\u5b66\u5206\u6790<\/p>\n<p>\u5728\u5b58\u5728\u7ade\u4e89\u53cd\u5e94\u8def\u5f84\u7684\u60c5\u51b5\u4e0b\uff0c\u4e0d\u540c\u7684\u5347\u6e29\u901f\u7387\u5f97\u5230\u7684\u7ec8\u4ea7\u7269\u7ec4\u6210\u53ef\u80fd\u4e0d\u540c<\/p>\n<p><a href=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/02\/\u6e29\u5ea6\u7684\u5f71\u54cd-2.jpg\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-68032\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/02\/\u6e29\u5ea6\u7684\u5f71\u54cd-2.jpg\" alt=\"\" width=\"364\" height=\"273\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/02\/\u6e29\u5ea6\u7684\u5f71\u54cd-2.jpg 364w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/02\/\u6e29\u5ea6\u7684\u5f71\u54cd-2-300x225.jpg 300w\" sizes=\"(max-width: 364px) 100vw, 364px\" \/><\/a><\/p>\n<p><strong>\u4e00\u822cDSC\u6d4b\u8bd5\u9700\u8981\u591a\u5c11\u6837\u54c1\uff0c\u6837\u54c1\u91cf\u5bf9DSC\u6d4b\u8bd5\u6709\u54ea\u4e9b\u5f71\u54cd\u5462\uff1f<\/strong><\/p>\n<p>\u5e76\u4e0d\u662f\u8bf4\u6837\u54c1\u91cf\u591a\u6216\u8005\u5c11\u5c31\u4e00\u5b9a\u597d\uff0c\u8fd9\u4e2a\u4e0e\u76ee\u6807\u5206\u6790\u7ed3\u679c\u6709\u5173<\/p>\n<table width=\"602\">\n<tbody>\n<tr style=\"height: 24px;\">\n<td style=\"text-align: center; height: 24px;\"><strong>\u6837\u54c1\u91cf\u5c0f<\/strong><\/td>\n<td style=\"text-align: center; height: 24px;\"><strong>\u6837\u54c1\u91cf\u5927<\/strong><\/td>\n<\/tr>\n<tr style=\"height: 24px;\">\n<td style=\"text-align: center; height: 24px;\">\u6240\u6d4b\u7279\u5f81\u6e29\u5ea6\u8f83\u4f4e\uff0c\u66f4\u201c\u771f\u5b9e\u201d<\/td>\n<td style=\"text-align: center; height: 24px;\">\u5cf0\u503c\u6e29\u5ea6\u5411\u9ad8\u6e29\u6f02\u79fb<\/td>\n<\/tr>\n<tr style=\"height: 24px;\">\n<td style=\"text-align: center; height: 24px;\">\u6709\u5229\u4e8e\u6c14\u4f53\u4ea7\u7269\u6269\u6563<\/td>\n<td style=\"text-align: center; height: 24px;\">\u00a0\u6837\u54c1\u5185\u6e29\u5ea6\u68af\u5ea6\u8f83\u5927\uff0c\u6c14\u4f53\u4ea7\u7269\u6269\u6563\u4ea6\u7a0d\u5dee<\/td>\n<\/tr>\n<tr style=\"height: 24px;\">\n<td style=\"text-align: center; height: 24px;\">\u76f8\u90bb\u5cf0\uff08\u5e73\u53f0\uff09\u5206\u79bb\u80fd\u529b\u589e\u5f3a<\/td>\n<td style=\"text-align: center; height: 24px;\">\u5cf0\u5206\u79bb\u80fd\u529b\u4e0b\u964d<\/td>\n<\/tr>\n<tr style=\"height: 24px;\">\n<td style=\"text-align: center; height: 24px;\">DSC \u5cf0\u5f62\u4e5f\u8f83\u5c0f<\/td>\n<td style=\"text-align: center; height: 24px;\">\u5cf0\u5f62\u52a0\u5bbd<\/td>\n<\/tr>\n<tr style=\"height: 24px;\">\n<td style=\"text-align: center; height: 24px;\">\u00a0\u2014\u2014\u2014\u2014\u2014\u2014\u2014\u2014\u2014\u2014\u2014\u2014<\/td>\n<td style=\"text-align: center; height: 24px;\">\u80fd\u589e\u5927 DSC \u68c0\u6d4b\u4fe1\u53f7<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p><a href=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/02\/\u6837\u54c1\u91cf\u7684\u5f71\u54cd.png\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-68036\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/02\/\u6837\u54c1\u91cf\u7684\u5f71\u54cd.png\" alt=\"\" width=\"511\" height=\"384\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/02\/\u6837\u54c1\u91cf\u7684\u5f71\u54cd.png 511w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/02\/\u6837\u54c1\u91cf\u7684\u5f71\u54cd-300x225.png 300w\" sizes=\"(max-width: 511px) 100vw, 511px\" \/><\/a><\/p>\n<ul>\n<li>\u4e00\u822c\u60c5\u51b5\u4e0b\uff0c\u4ee5\u8f83\u5c0f\u7684\u6837\u54c1\u91cf\u4e3a\u5b9c\u3002\u70ed\u5206\u6790\u5e38\u7528\u7684\u6837\u54c1\u91cf\u4e3a5\uff5e15mg\u3002<\/li>\n<\/ul>\n<ul>\n<li>\u5728\u6837\u54c1\u5b58\u5728\u4e0d\u5747\u5300\u6027\u7684\u60c5\u51b5\u4e0b\uff0c\u53ef\u80fd\u9700\u8981\u4f7f\u7528\u8f83\u5927\u7684\u6837\u54c1\u91cf\u624d\u5177\u6709\u4ee3\u8868\u6027\u3002<\/li>\n<\/ul>\n<p><strong>\u5728DSC\u6d4b\u8bd5\u8868\u5f81\u8fc7\u7a0b\u4e2d\uff0c\u5982\u4f55\u540c\u65f6\u9009\u62e9\u5408\u9002\u7684\u5347\u6e29\u901f\u7387\u548c\u6837\u54c1\u91cf\u5462\uff1f<\/strong><\/p>\n<p>\uff081\uff09\u63d0\u9ad8\u5bf9\u5fae\u5f31\u7684\u70ed\u6548\u5e94\u7684\u68c0\u6d4b\u7075\u654f\u5ea6\uff1a\u63d0\u9ad8\u5347\u6e29\u901f\u7387\uff0c\u52a0\u5927\u6837\u54c1\u91cf\uff1b<\/p>\n<p>\uff082\uff09\u63d0\u9ad8\u5fae\u91cf\u6210\u4efd\u7684\u70ed\u5931\u91cd\u68c0\u6d4b\u7075\u654f\u5ea6\uff1a\u52a0\u5927\u6837\u54c1\u91cf\uff1b<\/p>\n<p>\uff083\uff09\u63d0\u9ad8\u76f8\u90bb\u5cf0\uff08\u5931\u91cd\u5e73\u53f0\uff09\u7684\u5206\u79bb\u5ea6\uff1a\u6162\u901f\u5347\u6e29\u901f\u7387\uff0c\u5c0f\u7684\u6837\u54c1\u91cf\u3002<\/p>\n<p><strong>\u5bf9\u4e8e\u4e0d\u540c\u6761\u4ef6\u7684DSC\u6837\u54c1\uff0c\u5982\u4f55\u9009\u62e9\u5408\u9002\u7684\u5236\u6837\u65b9\u5f0f\uff1f<\/strong><\/p>\n<p>\uff081\uff09\u5757\u72b6\u6837\u54c1\uff1a\u5efa\u8bae\u5207\u6210\u8584\u7247\u6216\u788e\u7c92\uff1b<\/p>\n<p>\uff082\uff09\u7c89\u672b\u6837\u54c1\uff1a\u4f7f\u5176\u5728\u5769\u57da\u5e95\u90e8\u94fa\u5e73\u6210\u4e00\u8584\u5c42\uff1b<\/p>\n<p>\uff083\uff09\u5806\u79ef\u65b9\u5f0f\uff1a\u4e00\u822c\u5efa\u8bae\u5806\u79ef\u7d27\u5bc6\uff0c\u6709\u5229\u4e8e\u6837\u54c1\u5185\u90e8\u7684\u70ed\u4f20\u5bfc\uff1b\u5bf9\u4e8e\u6709\u5927\u91cf\u6c14\u4f53\u4ea7\u7269\u751f\u6210\u7684\u53cd\u5e94\uff0c\u53ef\u9002\u5f53\u758f\u677e\u5806\u79ef\u3002<\/p>\n<p><strong>DSC\u6d4b\u8bd5\u7684\u6c14\u6c1b\u5206\u54ea\u4e9b\u7c7b\uff0c\u6709\u4f55\u5e94\u7528\u533a\u522b\uff1f<\/strong><\/p>\n<p>\u6c14\u6c1b\u4e3b\u8981\u662f\u52a8\u6001\u6c14\u6c1b\u3001\u9759\u6001\u6c14\u6c1b\u548c\u771f\u7a7a3\u7c7b\uff0c\u53ef\u4ee5\u4ece\u4ee5\u4e0b\u4e09\u70b9\u6765\u5206\u522b<\/p>\n<p>\uff081\uff09\u4ece\u4fdd\u62a4\u5929\u5e73\u5ba4\u4e0e\u4f20\u611f\u5668\u3001\u9632\u6b62\u5206\u89e3\u7269\u6c61\u67d3\u7684\u89d2\u5ea6\uff0c\u4e00\u822c\u63a8\u8350\u4f7f\u7528\u52a8\u6001\u5439\u626b\u6c14\u6c1b\uff1b<\/p>\n<p>\uff082\uff09\u5bf9\u4e8e\u9ad8\u5206\u5b50TG\u6d4b\u8bd5\uff0c\u5728\u67d0\u4e9b\u573a\u5408\u4f7f\u7528\u771f\u7a7a\u6c14\u6c1b\uff0c\u80fd\u591f\u964d\u4f4e\u5c0f\u5206\u5b50\u6dfb\u52a0\u5242\u7684\u6cb8\u70b9\uff0c\u8fbe\u5230\u5206\u79bb\u5931\u91cd\u53f0\u9636\u7684\u76ee\u7684\uff1b<\/p>\n<p>\uff083\uff09\u82e5\u9700\u4f7f\u7528\u771f\u7a7a\u6216\u9759\u6001\u6c14\u6c1b\uff0c\u987b\u4fdd\u8bc1\u53cd\u5e94\u8fc7\u7a0b\u4e2d\u7684\u91ca\u51fa\u6c14\u4f53\u65e0\u5371\u5bb3\u6027\u3002<\/p>\n<p>\u5728\u4e0d\u540c\u7684\u6c14\u6c1b\u6761\u4ef6\u4e0b\uff0c\u7ed3\u679c\u6709\u65f6\u5019\u4e5f\u662f\u4e0d\u540c\u7684\uff0c\u6211\u4eec\u4e3e\u4e2a\u201c<b>NR\/SBR <\/b><b>\u6a61\u80f6\u4e2d\u589e\u5851\u5242\u7684\u5206\u89e3<\/b>\u201d\u7684\u4f8b\u5b50\uff1a<\/p>\n<p>\u5c06 NR\/SBR \u5171\u6df7\u6a61\u80f6\u6750\u6599\uff0c\u5728 N<sub>2<\/sub> \u6c14\u6c1b\u4e0b\u6309\u7167\u6807\u51c6\u7684 TG \u65b9\u6cd5\u8fdb\u884c\u5206\u6790\uff0c\u589e\u5851\u5242\u7684\u5931\u91cd\u91cf\u4e3a 9.87%\u3002\uff08\u589e\u5851\u5242\u5931\u91cd\u4e0e\u6a61\u80f6\u5206\u89e3\u53f0\u9636\u6709\u8f83\u5927\u91cd\u53e0\uff09<\/p>\n<p><a href=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/02\/N2\u6c14\u6c1b.jpg\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-68040\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/02\/N2\u6c14\u6c1b.jpg\" alt=\"\" width=\"521\" height=\"263\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/02\/N2\u6c14\u6c1b.jpg 521w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/02\/N2\u6c14\u6c1b-300x151.jpg 300w\" sizes=\"(max-width: 521px) 100vw, 521px\" \/><\/a><\/p>\n<p>\u5c06\u8be5\u6837\u54c1\u5728\u771f\u7a7a\u4e0b\u8fdb\u884c\u6d4b\u8bd5\uff0c\u7531\u4e8e\u589e\u5851\u5242\u6cb8\u70b9\u7684\u964d\u4f4e\uff0c\u6325\u53d1\u6e29\u5ea6\u4e0e\u6a61\u80f6\u5206\u89e3\u6e29\u5ea6\u62c9\u5f00\u8ddd\u79bb\uff0c\u5f97\u5230\u4e86\u66f4\u51c6\u786e\u7684\u589e\u5851\u5242\u8d28\u91cf\u767e\u5206\u6bd4\uff1a13.10%\u3002<\/p>\n<p><a href=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/02\/\u771f\u7a7a\u6c14\u6c1b.jpg\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-68041\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/02\/\u771f\u7a7a\u6c14\u6c1b.jpg\" alt=\"\" width=\"521\" height=\"266\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/02\/\u771f\u7a7a\u6c14\u6c1b.jpg 521w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/02\/\u771f\u7a7a\u6c14\u6c1b-300x153.jpg 300w\" sizes=\"(max-width: 521px) 100vw, 521px\" \/><\/a><\/p>\n<p><strong>DSC\u6d4b\u8bd5\u7684\u5e38\u7528\u6c14\u6c1b\u548c\u7279\u6b8a\u6c14\u6c1b\u6709\u54ea\u4e9b\uff1f<\/strong><\/p>\n<p>\u5e38\u7528\u6c14\u6c1b\uff1a<\/p>\n<p>N<sub>2<\/sub>: \u5e38\u7528\u60f0\u6027\u6c14\u6c1b<\/p>\n<p>Ar: \u60f0\u6027\u6c14\u6c1b\uff0c\u591a\u7528\u4e8e\u91d1\u5c5e\u6750\u6599\u7684\u9ad8\u6e29\u6d4b\u8bd5\u3002<\/p>\n<p>He: \u60f0\u6027\u6c14\u6c1b\uff0c\u56e0\u5176\u5bfc\u70ed\u6027\u597d\uff0c\u6709\u65f6\u7528\u4e8e\u4f4e\u6e29\u4e0b\u7684\u6d4b\u8bd5<\/p>\n<p>Air: \u6c27\u5316\u6027\u6c14\u6c1b\uff0c\u53ef\u4f5c\u53cd\u5e94\u6c14\u6c1b<\/p>\n<p>O<sub>2<\/sub>: \u5f3a\u6c27\u5316\u6027\u6c14\u6c1b\uff0c\u4e00\u822c\u7528\u4f5c\u53cd\u5e94\u6c14\u6c1b<\/p>\n<p>\u7279\u6b8a\u6c14\u6c1b\uff08\u5982H<sub>2<\/sub>\u3001CO\u3001HCl \u7b49\uff09\uff1a<\/p>\n<p>\u8003\u8651\u6c14\u6c1b\u5728\u6d4b\u8bd5\u6240\u8fbe\u5230\u7684\u6700\u9ad8\u6e29\u5ea6\u4e0b\u662f\u5426\u4f1a\u4e0e\u70ed\u7535\u5076\u3001\u5769\u57da\u7b49\u53d1\u751f\u53cd\u5e94\uff0c\u6ce8\u610f\u9632\u6b62\u7206\u70b8\u548c\u4e2d\u6bd2\u3002<\/p>\n<p>\u901a\u8fc7\u6539\u53d8\u6d4b\u8bd5\u6c14\u6c1b\uff08\u5982\u771f\u7a7a-\u6c2e\u6c14-\u7a7a\u6c14\uff09\uff0c\u6709\u52a9\u4e8e\u6df1\u5165\u5256\u6790\u6750\u6599\u6210\u5206\u3002<\/p>\n<p><strong>DSC\u90fd\u6709\u54ea\u4e9b\u5769\u57da\uff0c\u4ed6\u4eec\u6709\u4ec0\u4e48\u533a\u522b\uff1f<\/strong><\/p>\n<p>\u4e3a\u4e86\u9002\u5e94\u5343\u53d8\u4e07\u5316\u7684\u5404\u79cd\u6837\u54c1\uff0c\u907f\u514d\u6837\u54c1\u4e0e\u5769\u57da\u6750\u6599\u4e4b\u95f4\u7684\u4e0d\u76f8\u517c\u5bb9\uff0c\u8bbe\u5907\u4f9b\u5e94\u5546\u914d\u5907\u4e86\u591a\u79cd\u4e0d\u540c\u6750\u8d28\u4e0d\u540c\u7279\u70b9\u7684\u5769\u57da\uff0c\u5176\u4e2d\u51e0\u79cd\u5769\u57da\u56fe\u793a\u5982\u4e0b\uff1a<\/p>\n<p><a href=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/02\/\u56fe1-\u5769\u57da.png\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-68018\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/02\/\u56fe1-\u5769\u57da.png\" alt=\"\" width=\"600\" height=\"232\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/02\/\u56fe1-\u5769\u57da.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/02\/\u56fe1-\u5769\u57da-300x116.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/a><\/p>\n<p>\u5e38\u7528\u5769\u57da\uff1aAl, Al<sub>2<\/sub>O<sub>3<\/sub>, PtRh<\/p>\n<p>\u5176\u5b83\u5769\u57da\uff1aPtRh+Al<sub>2<\/sub>O<sub>3<\/sub>,\u00a0\u00a0 Steel, Cu, Graphite, ZrO<sub>2<\/sub>, Ag, Au, Quartz \u7b49<\/p>\n<p>\u538b\u529b\u5769\u57da\uff1a\u4e2d\u538b\u5769\u57da\uff0c\u9ad8\u538b\u5769\u57da<\/p>\n<table style=\"width: 616px;\">\n<tbody>\n<tr style=\"height: 176px;\">\n<td style=\"width: 96px; height: 176px;\">Al\u5769\u57da<\/td>\n<td style=\"width: 532px; height: 176px;\">\n<p>\u4f20\u70ed\u6027\u597d\uff0c\u7075\u654f\u5ea6\u3001\u5cf0\u5206\u79bb\u80fd\u529b\u3001\u57fa\u7ebf\u6027\u80fd\u7b49\u5747\u4f73<\/p>\n<p>\u6e29\u5ea6\u8303\u56f4\u8f83\u7a84\uff08&lt; 600\u2103\uff09<\/p>\n<p>\u7528\u4e8e\u4e2d\u4f4e\u6e29\u578bDSC\u6d4b\u8bd5<\/p>\n<p>\u53ef\u7528\u4e8e\u6bd4\u70ed\u6d4b\u8bd5<\/p>\n<\/td>\n<\/tr>\n<tr style=\"height: 24px;\">\n<td style=\"width: 96px; height: 24px;\">PtRh \u5769\u57da<\/td>\n<td style=\"width: 532px; height: 24px;\">\n<p>\u4f20\u70ed\u6027\u597d\uff0c\u7075\u654f\u5ea6\u9ad8\u3001\u5cf0\u5206\u79bb\u80fd\u529b\u3001\u57fa\u7ebf\u6027\u80fd\u4f73<\/p>\n<p>\u6e29\u5ea6\u8303\u56f4\u5bbd\u5e7f<\/p>\n<p>\u9002\u4e8e\u7cbe\u786e\u6d4b\u91cf\u6bd4\u70ed<\/p>\n<p><strong>\u6613\u4e0e\u7194\u5316\u7684\u91d1\u5c5e\u6837\u54c1\u5f62\u6210\u5408\u91d1<\/strong><\/p>\n<p>\u6e05\u6d17\u4e0e\u56de\u6536\uff1a\u53ef\u4f7f\u7528\u6c22\u6c1f\u9178\u6d78\u6ce1\u6e05\u6d17<\/p>\n<\/td>\n<\/tr>\n<tr style=\"height: 24px;\">\n<td style=\"width: 96px; height: 24px;\">Al<sub>2<\/sub>O<sub>3<\/sub> \u5769\u57da<\/td>\n<td style=\"width: 532px; height: 24px;\">\n<p>\u6837\u54c1\u9002\u5e94\u9762\u5e7f\uff0c\u5176\u7075\u654f\u5ea6\u3001\u5cf0\u5206\u79bb\u80fd\u529b\u3001\u57fa\u7ebf\u6f02\u79fb\u7b49\u8f83PtRh\u5dee<\/p>\n<p>\u6e29\u5ea6\u8303\u56f4\u5bbd\u5e7f\uff08\u53ef\u7528\u4e8e\u9ad8\u6e291650\u2103 \uff09<\/p>\n<p>\u4e0d\u9002\u4e8e\u6d4b\u5b9a\u6bd4\u70ed<\/p>\n<p><b>\u6613\u4e0e\u90e8\u5206\u65e0\u673a\u7194\u878d\u6837\u54c1\uff08\u5982\u7845\u9178\u76d0\u3001\u6c27\u5316\u94c1\u7b49\uff09\u53cd\u5e94\u6216\u6269\u6563\u6e17\u900f<\/b><\/p>\n<p><b>\u6e05\u6d17\u4e0e\u56de\u6536\uff1a\u53ef\u4f7f\u7528\u738b\u6c34\u4e0e\u6c28\u6c34\u6d78\u6ce1\u6e05\u6d17<\/b><\/p>\n<\/td>\n<\/tr>\n<tr style=\"height: 24px;\">\n<td style=\"width: 96px; height: 24px;\">Cu\u5769\u57da<\/td>\n<td style=\"width: 532px; height: 24px;\">\n<p>\u5bf9\u5851\u6599\u7684\u6c27\u5316\u6709\u50ac\u5316\u4f5c\u7528\uff0c\u6709\u65f6\u7528\u4e8e\u6c27\u5316\u8bf1\u5bfc\u671f\uff08O.I.T.\uff09\u6d4b\u8bd5<\/p>\n<\/td>\n<\/tr>\n<tr style=\"height: 24px;\">\n<td style=\"width: 96px; height: 24px;\">\u4e2d\u538b\u4e0e\u9ad8\u538b\u5769\u57da<\/td>\n<td style=\"width: 532px; height: 24px;\">\u9002\u7528\uff1a\u6325\u53d1\u6027\u6db2\u4f53\u6837\u54c1\uff0c\u6db2\u76f8\u53cd\u5e94\uff0c\u9700\u8981\u7ef4\u6301\u6c14\u4f53\u5206\u538b\u7684\u5c01\u95ed\u4f53\u7cfb\u53cd\u5e94<\/p>\n<p>\u4e2d\u538b\u5769\u57da\u6700\u9ad8\u4f7f\u7528\u538b\u529b20bar<\/p>\n<p>\u9ad8\u538b\u5769\u57da\u4e3a100bar<\/p>\n<p>\u6e29\u5ea6\u8f83\u4f4e\u3001\u6325\u53d1\u7269\u538b\u529b\u4e0d\u592a\u5927\u65f6\uff0c\u53ef\u7528\u5bc6\u95ed\u538b\u5236\u7684Al\u5769\u57da\u4ee3\u66ff<\/p>\n<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p>DSC\u6d4b\u8bd5\u4e2d\u5769\u57da\u52a0\u76d6\u4e0e\u5426\u5982\u4f55\u9009\u62e9\uff1f<\/p>\n<p>\u9996\u5148\u8981\u77e5\u9053\u5769\u57da\u52a0\u76d6\u7684\u4f18\u7f3a\u70b9\u4ee5\u53ca\u5769\u57da\u76d6\u624e\u5b54\u7684\u76ee\u7684<\/p>\n<table style=\"height: 126px;\" width=\"634\">\n<tbody>\n<tr>\n<td style=\"width: 204px; text-align: center;\"><strong>\u4f18\u70b9<\/strong><\/td>\n<td style=\"width: 204px; text-align: center;\"><strong>\u7f3a\u70b9<\/strong><\/td>\n<td style=\"width: 204px; text-align: center;\"><strong>\u624e\u5b54\u7684\u76ee\u7684<\/strong><\/td>\n<\/tr>\n<tr>\n<td style=\"width: 204px;\">\u6709\u5229\u4e8e\u4f53\u7cfb\u5185\u90e8\u6e29\u5ea6\u5747\u5300<\/td>\n<td style=\"width: 204px;\">\u51cf\u5c11\u4e86\u53cd\u5e94\u6c14\u6c1b\u4e0e\u6837\u54c1\u7684\u63a5\u89e6<\/td>\n<td style=\"width: 204px;\">\u4fdd\u8bc1\u6837\u54c1\u4e0e\u6c14\u6c1b\u4e00\u5b9a\u63a5\u89e6<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 204px;\">\u51cf\u5c11\u8f90\u5c04\u6548\u5e94\u4e0e\u6837\u54c1\u989c\u8272\u7684\u5f71\u54cd<\/td>\n<td style=\"width: 204px;\">\u4ea7\u7269\u6c14\u4f53\u4e0d\u6613\u5e26\u8d70<\/td>\n<td style=\"width: 204px;\">\u5141\u8bb8\u4e00\u5b9a\u7a0b\u5ea6\u7684\u6c14\u56fa\u53cd\u5e94<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 204px;\">\u9632\u6b62\u5fae\u7ec6\u6837\u54c1\u7c89\u672b\u98de\u626c\uff0c\u6216\u5728\u62bd\u53d6\u771f\u7a7a\u8fc7\u7a0b\u4e2d\u88ab\u5e26\u8d70<\/td>\n<td style=\"width: 204px;\">\u5bfc\u81f4\u53cd\u5e94\u4f53\u7cfb\u538b\u529b\u8f83\u9ad8<\/td>\n<td style=\"width: 204px;\">\u5141\u8bb8\u6c14\u4f53\u4ea7\u7269\u968f\u52a8\u6001\u6c14\u6c1b\u5e26\u8d70<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 204px;\">\u6709\u6548\u9632\u6b62\u4f20\u611f\u5668\u53d7\u5230\u6c61\u67d3<\/td>\n<td style=\"width: 204px;\">\u00a0<\/td>\n<td style=\"width: 204px;\">\u00a0 \u4fdd\u6301\u5769\u57da\u5185\u5916\u538b\u529b\u5e73\u8861<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p>\uff081\uff09\u7269\u7406\u6548\u5e94\u6d4b\u8bd5\uff08\u7194\u878d\u3001\u7ed3\u6676\u3001\u76f8\u53d8\u7b49DSC\u6d4b\u8bd5\uff09\uff0c\u901a\u5e38\u9009\u62e9\u52a0\u76d6\u5769\u57da\uff1b<\/p>\n<p>\uff082\uff09\u672a\u77e5\u6837\u54c1\uff0c\u51fa\u4e8e\u5b89\u5168\u6027\u8003\u8651\uff0c\u901a\u5e38\u9009\u62e9\u52a0\u76d6\u5769\u57da\uff1b<\/p>\n<p>\uff083\uff09\u6c14\u56fa\u53cd\u5e94\uff08\u5982\u6c27\u5316\u8bf1\u5bfc\u671f\u6d4b\u8bd5\u6216\u5438\u9644\u53cd\u5e94\uff09\uff0c\u4f7f\u7528\u4e0d\u52a0\u76d6\u655e\u53e3\u5769\u57da\uff1b<\/p>\n<p>\uff084\uff09\u6db2\u76f8\u53cd\u5e94\uff0c\u6613\u6325\u53d1\u6837\u54c1\uff0c\u4f7f\u7528\u52a0\u76d6\u538b\u5236Al \u5769\u57da\u3001\u4e2d\u538b\u6216\u9ad8\u538b\u5769\u57da\uff1b<\/p>\n<p>\uff085\uff09\u6709\u6c14\u4f53\u751f\u6210\u7684\u53cd\u5e94\uff08\u5305\u62ec\u591a\u6570\u5206\u89e3\u53cd\u5e94 \uff09\u6216\u504f\u91cd\u4e8e TG \u7684\u6d4b\u8bd5\uff0c\u5728\u4e0d\u6c61\u67d3\u635f\u5bb3\u6837\u54c1\u652f\u67b6\u7684\u524d\u63d0\u4e0b\uff0c\u6839\u636e\u5b9e\u9a8c\u9700\u8981\uff0c\u8fdb\u884c\u52a0\u76d6\u4e0e\u5426\u7684\u9009\u62e9\u3002<\/p>\n<p><strong>\u5982\u4f55\u6d4b\u8bd5\u4e00\u4e9b\u8f83\u5fae\u5f31\u7684\u3001\u5728\u5e38\u89c4\u6761\u4ef6\u4e0b\u4e0d\u6613\u6d4b\u51fa\u7684\u73bb\u7483\u5316\u8f6c\u53d8\uff1f\u00a0<\/strong><\/p>\n<p>\u6309\u7167\u4e00\u822c\u7684\u70ed\u5206\u6790\u89c4\u5f8b\uff0c\u53ef\u8003\u8651\u52a0\u5927\u6837\u54c1\u91cf\u4e0e\u4f7f\u7528\u8f83\u5feb\u4e00\u4e9b\u7684\u5347\u6e29\u901f\u7387\u3002<\/p>\n<p>\u5bf9\u4e8e\u534a\u7ed3\u6676\u6027\u7684\u9ad8\u5206\u5b50\u6750\u6599\uff0c\u54b1\u4eec\u4e09\u6b65\u8d70\uff1a<\/p>\n<p>\uff081\uff09\u5148\u5347\u8fc7\u7194\u70b9\u4f7f\u6837\u54c1\u5145\u5206\u7194\u878d\uff1b<\/p>\n<p>\uff082\uff09\u968f\u540e\u6dec\u51b7\u81f3\u73bb\u7483\u5316\u6e29\u5ea6\u4ee5\u4e0b\uff1b<\/p>\n<p>\uff083\uff09 \u518d\u6b21\u5347\u6e29\u65f6\u73bb\u7483\u5316\u8f6c\u53d8\u8f83\u4e3a\u660e\u663e.<\/p>\n<p><b>\u4f7f\u7528\u6db2\u6c2e\u8fdb\u884c\u51b7\u5374\u7684\u964d\u6e29\u6d4b\u8bd5\uff0c\u5982\u4f55\u4f7f\u6e29\u5ea6\u66f2\u7ebf\u5c3d\u5feb\u8fbe\u5230\u7ebf\u6027\uff1f<\/b><\/p>\n<p>\u5728\u964d\u6e29\u6bb5\u4e4b\u524d\u8bbe\u7f6e\u4e00\u4e2a\u6052\u6e29\u6bb5\uff08\u4e00\u822c5\uff5e10min\u5de6\u53f3\uff09\uff0c\u5c06LN\u6253\u5f00\uff0c\u521d\u59cb\u6d41\u91cf\u4e0d\u9700\u5f88\u5927\uff0c\u8ba9\u4eea\u5668\u5728\u964d\u6e29\u4e4b\u524d\u5148\u9002\u5e94\u4e00\u4e0bLN\u3002\u7136\u540e\u964d\u6e29\u6bb5\u8bbe\u7f6e\u7684\u6d41\u91cf\u6839\u636e\u60c5\u51b5\u914c\u60c5\u52a0\u5927\u4e00\u4e9b\uff0c\u4f46\u65e0\u9700\u5f00\u5230\u6700\u5927\uff0c\u4eea\u5668\u4f1a\u81ea\u52a8\u6839\u636e\u51b7\u5374\u9700\u8981\u8c03\u8282\u6db2\u6c2e\u6d41\u91cf\u3002\u8fd9\u6837\u5c31\u80fd\u4f7f\u51b7\u5374\u6e29\u5ea6\u7ebf\u8f83\u5feb\u7684\u8fbe\u5230\u7ebf\u6027\u3002<\/p>\n<p><b>\u94dd\u5769\u57da\u7684\u52a0\u76d6\u4e0e\u538b\u5236\u6709\u54ea\u4e9b\u5b9e\u9a8c\u6280\u5de7\uff1f<\/b><\/p>\n<p>\uff081\uff09\u5769\u57da\u76d6\u5b50\u624e\u5b54\u5bc6\u95ed\uff1a\u8fd9\u662f\u5e38\u89c4\u7684\u5769\u57da\u4f7f\u7528\u65b9\u6cd5\uff0c\u5b83\u9002\u7528\u4e8e\u56fa\u4f53\u6d4b\u8bd5\uff0c\u6837\u54c1\u53ef\u4ee5\u7c89\u672b\uff0c\u9897\u7c92\uff0c\u7247\u72b6\uff0c\u5757\u72b6\u7b49\u7b49\u3002<\/p>\n<p>\uff082\uff09\u5769\u57da\u76d6\u5b50\u624e\u5b54\uff0c\u4e0d\u5bc6\u95ed\uff1a\u8fd9\u79cd\u65b9\u6cd5\u662f\u4e00\u79cd\u6bd4\u8f83\u7ecf\u6d4e\u7684\u65b9\u6cd5\uff0c\u5bf9\u4e8e\u8282\u7701\u5769\u57da\u635f\u8017\u5f88\u6709\u5e2e\u52a9\u3002\u6709\u4e9b\u6837\u54c1\u505a\u5b8c\u8bd5\u9a8c\u540e\u53ef\u4ee5\u53d6\u51fa\u6765\u4e14\u4e0d\u6c61\u67d3\u5769\u57da\uff0c\u6211\u4eec\u53ef\u4ee5\u91c7\u53d6\u8fd9\u79cd\u65b9\u6cd5\uff0c\u4e0d\u7528\u538b\u673a\u5c06\u5769\u57da\u76d6\u5b50\u548c\u5e73\u76d8\u538b\u6b7b\uff0c\u8fd9\u6837\u5769\u57da\u5c31\u53ef\u4ee5\u91cd\u590d\u4f7f\u7528\u4e86\u3002<\/p>\n<p>\uff083\uff09\u655e\u53e3\u5769\u57da\uff1a\u5373\u4e0d\u52a0\u5769\u57da\u76d6\u5b50\uff0c\u5b83\u9002\u7528\u4e8e\u9700\u8981\u4e0e\u5439\u626b\u6c14\u6c1b\u5145\u5206\u63a5\u89e6\u7684\u5b9e\u9a8c\uff08\u5982\u6c27\u5316\u8bf1\u5bfc\u671f\u6d4b\u8bd5\uff09\uff0c\u4f46\u7531\u4e8e\u6837\u54c1\u8868\u9762\u4e0e\u6d41\u52a8\u6c14\u4f53\u63a5\u89e6\u4f1a\u5e26\u8d70\u4e00\u5b9a\u7684\u70ed\u91cf\uff0c\u91cf\u70ed\u7cbe\u5ea6\u4f1a\u7a0d\u4f4e\u4e00\u4e9b\u3002<\/p>\n<p>\uff084\uff09\u5769\u57da\u5bc6\u95ed\uff1a\u5769\u57da\u76d6\u5b50\u4e0d\u624e\u5b54\uff0c\u7528\u538b\u673a\u5c06\u5769\u57da\u7262\u7262\u5bc6\u5c01\u4f4f\uff0c\u5b83\u9002\u7528\u4e8e\u5e38\u89c4\u7684\u6db2\u4f53\u6d4b\u8bd5\u3002\u5bf9\u4e8e\u4e00\u4e9b\u9700\u8981\u5b8c\u5168\u5bc6\u95ed\uff0c\u80fd\u627f\u53d7\u66f4\u9ad8\u538b\u529b\u7684\u6d4b\u8bd5\uff0c\u8010\u9a70\u8fd8\u63d0\u4f9b\u4e13\u95e8\u7684\u4e2d\u538b\u3001\u9ad8\u538b\u5769\u57da\u3002<\/p>\n<p><strong>DSC\u5728\u64cd\u4f5c\u8fc7\u7a0b\u4e2d\u6709\u54ea\u4e9b\u8981\u7279\u522b\u6ce8\u610f\u7684\u5730\u65b9\uff1f<\/strong><\/p>\n<p>\uff081\uff09\u4eea\u5668\u53ef\u4e00\u76f4\u5904\u4e8e\u5f00\u673a\u72b6\u6001\uff0c\u5c3d\u91cf\u907f\u514d\u9891\u7e41\u5f00\u673a\u5173\u673a<\/p>\n<p>\uff082\uff09\u4eea\u5668\u5e94\u81f3\u5c11\u63d0\u524d1\u5c0f\u65f6\u5f00\u673a<\/p>\n<p>\uff083\uff09\u5c3d\u91cf\u907f\u514d\u5728\u4eea\u5668\u6781\u9650\u6e29\u5ea6\u9644\u8fd1\u8fdb\u884c\u6052\u6e29\u64cd\u4f5c<\/p>\n<p>\uff084\uff09\u8bd5\u9a8c\u5b8c\u6210\u540e\uff0c\u5fc5\u987b\u7b49\u7089\u6e29\u964d\u5230200\u00b0C\u4ee5\u4e0b\u540e\u624d\u80fd\u6253\u5f00\u7089\u4f53<\/p>\n<p>\uff085\uff09\u6d4b\u8bd5\u6837\u54c1\u53ca\u5176\u5206\u89e3\u7269\u4e0d\u80fd\u5bf9\u4f20\u611f\u5668\u3001\u70ed\u7535\u5076\u9020\u6210\u6c61\u67d3<\/p>\n<p>\u5177\u4f53\u63aa\u65bd\uff1a\u5b9e\u9a8c\u524d\u5e94\u5bf9\u6837\u54c1\u7684\u7ec4\u6210\u6709\u5927\u81f4\u4e86\u89e3\uff0c\u5982\u6709\u5371\u5bb3\u6027\u6c14\u4f53\u4ea7\u751f\uff0c\u5b9e\u9a8c\u8981\u52a0\u5927\u5439\u626b\u6c14\u7684\u7528\u91cf<\/p>\n<p>\uff086\uff09\u6d4b\u8bd5\u6837\u54c1\u53ca\u5176\u5206\u89e3\u7269\u7edd\u5bf9\u4e0d\u80fd\u4e0e\u6d4b\u91cf\u5769\u9505\u53d1\u751f\u53cd\u5e94\uff0c\u5177\u4f53\u4e3a\uff1a<\/p>\n<p>\u94dd\u5769\u9505\u6d4b\u8bd5\uff0c\u6d4b\u8bd5\u7ec8\u6b62\u6e29\u5ea6\u4e0d\u80fd\u8d85\u8fc7600\u00b0C\uff1b<\/p>\n<p>\u7edd\u5bf9\u907f\u514d\u4f7f\u7528\u94c2\u5769\u9505\u8fdb\u884c\u6d4b\u8bd5\u91d1\u5c5e\u6837\u54c1\uff1b<\/p>\n<p>\u91d1\u5c5e\u6837\u54c1\u7684\u6d4b\u8bd5\u9700\u67e5\u84b8\u6c14\u538b\uff5e\u6e29\u5ea6\u8868\u683c\u3002<\/p>\n<p><strong>\u7089\u4f53\u5982\u679c\u5df2\u53d1\u751f\u6c61\u67d3\uff0c\u8be5\u5982\u4f55\u5904\u7406\uff1f<\/strong><\/p>\n<p><b><\/b>\uff081\uff09\u4f7f\u7528\u68c9\u82b1\u68d2\u8638\u4e0a\u9152\u7cbe\u8f7b\u8f7b\u64e6\u6d17\uff1b<\/p>\n<p>\uff082\uff09\u4f7f\u7528\u5927\u6d41\u91cf\u60f0\u6027\u5439\u626b\u6c14\u6c1b\u7a7a\u70e7\u81f3600\u2103\uff1b<\/p>\n<p>\uff083\uff09\u5728\u65e5\u5e38\u4f7f\u7528\u6e29\u5ea6\u8303\u56f4\u5185\u8fdb\u884c\u57fa\u7ebf\u7684\u9a8c\u8bc1\u6d4b\u8bd5\uff0c\u82e5\u57fa\u7ebf\u6b63\u5e38\u65e0\u5cf0\uff0c\u4f20\u611f\u5668\u4e00\u822c\u4ecd\u53ef\u7ee7\u7eed\u4f7f\u7528\uff1b<\/p>\n<p>\uff084\uff09\u4f7f\u7528\u6807\u6837In\u4e0eZn\u8fdb\u884c\u6e29\u5ea6\u4e0e\u7075\u654f\u5ea6\u7684\u9a8c\u8bc1\u6d4b\u8bd5\uff0c\u82e5\u6e29\u5ea6\u4e0e\u70ed\u7113\u8f83\u7406\u8bba\u503c\u53d1\u751f\u4e86\u8f83\u5927\u504f\u5dee\uff0c\u9700\u8981\u91cd\u65b0\u8fdb\u884c\u6821\u6b63\u3002<\/p>\n<p><strong>\u5728\u54ea\u91cc\u53ef\u4ee5\u83b7\u5f97\u9ad8\u8d28\u91cf\u7684DSC\u6d4b\u8bd5\u8868\u5f81\uff1f<\/strong><\/p>\n<p>\u6750\u6599\u4eba\u6d4b\u8bd5\u8c37\uff08www.ceshigu.com\uff09\u63d0\u4f9b\u9ad8\u8d28\u91cf\u6750\u6599\u8868\u5f81\u670d\u52a1\uff0c\u8fd8\u63d0\u4f9b\u4e13\u4e1a\u57f9\u8bad\u3001\u79d1\u7814\u5236\u56fe\u3001\u8bba\u6587\u6da6\u8272\u3001DFT\u8ba1\u7b97\u7b49\u670d\u52a1\u3002<strong>\u6e05\u534e\u5927\u5b66\u6df1\u5733\u7814\u7a76\u751f\u9662\u6750\u6599\u4e0e\u5668\u4ef6\u68c0\u6d4b\u4e2d\u5fc3<\/strong>1\u4ebf\u8bbe\u5907\u7387\u5148\u5165\u9a7b\uff0c\u5404\u5927\u68c0\u6d4b\u4e2d\u5fc3\u3001\u5b9e\u9a8c\u5ba4\u4ee5\u53ca\u8eab\u6000\u7edd\u6280\u7684\u5c0f\u4f19\u4f34\u4eec\uff0c\u8fd8\u5728\u7b49\u4ec0\u4e48\uff0c\u5feb\u5230\u7897\u91cc\u6765\uff01<\/p>\n<p>\u60a8\u53ef\u4ee5\u8fdb\u5165\u6d4b\u8bd5\u8c37\u5b98\u7f51www.ceshigu.com\uff0c\u6216\u901a\u8fc7\u5173\u6ce8\u6d4b\u8bd5\u8c37\u5fae\u4fe1\u516c\u4f17\u53f7\uff08ceshigu_online\uff09\u6216\u8005\u52a0\u6d4b\u8bd5\u8c37\u5fae\u4fe1\uff08iceshigu\uff09\u8054\u7cfb\u6211\u4eec\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u8bf7\u8bb2\u4e00\u8bb2DSC\u57fa\u672c\u539f\u7406\u4e0e\u7ecf\u5178\u5e94\u7528\uff1f \u5728\u7a0b\u5e8f\u6e29\u5ea6\uff08\u5347\uff0f\u964d\uff0f\u6052\u6e29\u53ca\u5176\u7ec4\u5408\uff09\u8fc7\u7a0b\u4e2d\uff0c\u6d4b\u91cf\u6837\u54c1\u4e0e\u53c2\u8003\u7269\u4e4b\u95f4\u7684\u70ed\u6d41\u5dee\uff0c\u4ee5\u8868\u5f81\u6240\u6709\u4e0e\u70ed\u6548\u5e94\u6709\u5173\u7684\u7269\u7406\u53d8\u5316\u548c\u5316\u5b66\u53d8\u5316\u3002 \u5178\u578b\u5e94&#8230;<\/p>\n","protected":false},"author":51,"featured_media":68041,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[4],"tags":[2513],"class_list":["post-68013","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-ganhuo","tag-refenxi"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/68013"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/51"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=68013"}],"version-history":[{"count":9,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/68013\/revisions"}],"predecessor-version":[{"id":68687,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/68013\/revisions\/68687"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/68041"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=68013"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=68013"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=68013"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}