{"id":71569,"date":"2017-03-16T06:30:48","date_gmt":"2017-03-15T22:30:48","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=71569"},"modified":"2017-10-17T23:15:20","modified_gmt":"2017-10-17T15:15:20","slug":"%e4%b8%8d%e5%be%97%e4%b8%8d%e8%b5%9e%ef%bc%81%e8%b6%85%e5%ae%9e%e7%94%a8%e7%9a%84%e5%b8%b8%e8%a7%81%e6%9d%90%e6%96%99%e5%88%86%e6%9e%90%e6%b5%8b%e8%af%95%e7%a7%8d%e7%b1%bb%e3%80%81%e5%9e%8b%e5%8f%b7","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=71569","title":{"rendered":"\u4e0d\u5f97\u4e0d\u8d5e\uff01\u8d85\u5b9e\u7528\u7684\u5e38\u89c1\u6750\u6599\u5206\u6790\u6d4b\u8bd5\u79cd\u7c7b\u3001\u578b\u53f7\u53ca\u53ef\u6d4b\u6027\u80fd"},"content":{"rendered":"<p>\u6c89\u8ff7\u79d1\u7814\u7684\u4f60\u53ef\u80fd\u9700\u8981\u4e00\u6b21\u5bf9\u5e38\u7528\u4eea\u5668\u4fe1\u606f\u3001\u5e38\u89c1\u578b\u53f7\u4ee5\u53ca\u53ef\u6d4b\u53c2\u6570\u7b80\u5355\u7c97\u66b4\u7684\u79d1\u666e\uff0c\u6765\uff0c\u6536\u4e0b\u8fd9\u4efd\u5e72\u8d27\uff01<\/p>\n<p>\u968f\u540e\u5c0f\u7f16\u5c06\u901a\u8fc7\u5bf9\u6bd4\u7684\u65b9\u5f0f\u4ecb\u7ecd\u5404\u79cd\u8868\u5f81\u65b9\u5f0f\u7684\u5f02\u540c\uff0c\u4e00\u8d77\u63a2\u8ba8\u5982\u4f55\u73a9\u8f6c\u8fd9\u6d4b\u8bd5\u5206\u6790\u7684\u5341\u516b\u822c\u6b66\u5668\u3002<\/p>\n<p>\u4e0d\u4ec5\u5982\u6b64\uff0c\u4ee5\u4e0b\u6d4b\u8bd5\uff0c\u6750\u6599\u4eba\u6d4b\u8bd5\u8c37\u90fd\u80fd\u9ad8\u8d28\u91cf\u5b8c\u6210\uff0c\u53e6\u5916\u8fd8\u80fd\u63d0\u4f9b\u4e00\u4e9b\u975e\u5e38\u89c4\u7684\u6d4b\u8bd5\uff0c\u5982\u7403\u5dee\u7535\u955c\u3001\u626b\u63cf\u96a7\u9053\u663e\u5fae\u955c\u3001\u7a46\u65af\u5821\u5c14\u8c31\u3001\u6781\u4f4e\u6e29\u7269\u6027\u6d4b\u8bd5\/\u70ed\u5bfc\/\u529b\u5b66\u6027\u80fd\u7b49\u3002<\/p>\n<p>\u5bf9\u4e8e\u6d4b\u8bd5\u8868\u5f81\u4e4b\u540e\u7684\u6570\u636e\u5206\u6790\u3001XRD\u7cbe\u4fee\u3001\u8bba\u6587\u6da6\u8272\u548c\u79d1\u7814\u5236\u56fe\uff0c\u6211\u4eec\u4e5f\u4e3a\u5927\u5bb6\u51c6\u5907\u5927\u91cf\u7684\u4f18\u79c0\u5de5\u7a0b\u5e08\u548c\u57f9\u8bad\u6559\u7a0b\uff0c\u8bb0\u5f97\u5173\u6ce8\u6211\u4eec\u8fd1\u671f\u63a8\u51fa\u76843Dmax\u7cfb\u5217\u8bb2\u5ea7\u54e6\uff0c16\u8282\u8bfe\u4e0d\u5bb9\u9519\u8fc7\uff01<\/p>\n<hr \/>\n<p><strong><span style=\"color: #3366ff;\">\u539f\u5b50\u529b\u663e\u5fae\u955c\uff08AFM\uff09<\/span><\/strong><\/p>\n<table style=\"width: 100%;\">\n<tbody>\n<tr style=\"height: 56px;\">\n<td style=\"width: 184px; height: 224px;\" rowspan=\"4\">\n<p style=\"text-align: center;\">\u539f\u5b50\u529b\u663e\u5fae\u955c<\/p>\n<\/td>\n<td style=\"width: 339px; height: 224px;\" rowspan=\"4\">\n<p style=\"text-align: center;\">Bruker dimension icon<\/p>\n<\/td>\n<td style=\"width: 224px; height: 56px;\">\n<p style=\"text-align: center;\">\u57fa\u672c\u5f62\u8c8c\u30013D\u6548\u679c\u663e\u793a<\/p>\n<\/td>\n<\/tr>\n<tr style=\"height: 56px;\">\n<td style=\"width: 224px; height: 56px; text-align: center;\">\n<p>\u7535\u5b66\u78c1\u5b66\u529b\u5b66<\/p>\n<\/td>\n<\/tr>\n<tr style=\"height: 56px;\">\n<td style=\"width: 224px; height: 56px; text-align: center;\">\n<p>\u70ed\u5b66<\/p>\n<\/td>\n<\/tr>\n<tr style=\"height: 56px;\">\n<td style=\"width: 224px; height: 56px; text-align: center;\">\n<p>\u7c97\u7cd9\u5ea6\u5206\u6790<\/p>\n<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p><span style=\"color: #3366ff;\"><strong>\u00a0\u900f\u5c04\u7535\u5b50\u663e\u5fae\u955c\uff08TEM\uff09<\/strong><\/span><\/p>\n<table style=\"width: 100%;\">\n<tbody>\n<tr>\n<td style=\"width: 183px; text-align: center;\" rowspan=\"12\">\n<p>\u900f\u5c04\u7535\u5b50\u663e\u5fae\u955c<\/p>\n<\/td>\n<td style=\"width: 338px; text-align: center;\" rowspan=\"12\">\n<p>JEM2100F<\/p>\n<p>FEI Tecnai G2 F30<\/p>\n<p>Tecnai G2 Spirit120KV<\/p>\n<p>Titan Cubed Themis G2 300<\/p>\n<p>Titan 80-300<\/p>\n<p>JEM-2010F<\/p>\n<p>EI Tecnai G2 20<\/p>\n<\/td>\n<td style=\"width: 229px; text-align: center;\">\n<p>TEM\u5f62\u8c8c\u89c2\u5bdf<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 229px; text-align: center;\">\n<p>HRTEM\u9ad8\u5206\u8fa8\u50cf<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 229px; text-align: center;\">\n<p>EDS\u80fd\u8c31\u5143\u7d20\u5b9a\u6027\u5b9a\u91cf\u5206\u6790<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 229px; text-align: center;\">\n<p>STEM\u626b\u63cf\u900f\u5c04\u7535\u5b50\u663e\u5fae\u56fe\u50cf<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 229px; text-align: center;\">\n<p>EELS\u80fd\u91cf\u635f\u5931\u8c31<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 229px; text-align: center;\">\n<p>SAED\u9009\u533a\u7535\u5b50\u884d\u5c04<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 229px; text-align: center;\">\n<p>S\/TEM\u3001EDS\u4e09\u7ef4\u91cd\u6784<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 229px; text-align: center;\">\n<p>\u5fae\u5206\u76f8\u4f4d\u886c\u5ea6STEM\u6280\u672f\u6d4b\u91cf\u56fa\u6709\u78c1\u573a\u548c\u7535\u573a<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 229px; text-align: center;\">\n<p>\u5168\u606f\u6280\u672f<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 229px; text-align: center;\">\n<p>\u7f3a\u9677\u5206\u6790<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 229px; text-align: center;\">\n<p>\u7ed3\u6784\u6d4b\u5b9a<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 229px; text-align: center;\">\n<p>\u6d1b\u4f26\u5179\u900f\u955c<\/p>\n<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p><strong><span style=\"color: #3366ff;\">\u00a0\u626b\u63cf\u7535\u5b50\u663e\u5fae\u955c-SEM<\/span><\/strong><\/p>\n<table style=\"width: 100%;\">\n<tbody>\n<tr>\n<td style=\"width: 184px; text-align: center;\" rowspan=\"8\">\n<p>\u573a\u53d1\u5c04\u626b\u63cf\u7535\u5b50\u663e\u5fae\u955c<\/p>\n<\/td>\n<td style=\"width: 336px; text-align: center;\" rowspan=\"8\">\n<p>Zeiss Merlin<\/p>\n<p>Hitachi SU8010<\/p>\n<p>Hitachi S-3400N<\/p>\n<p>\u65e5\u7acbS-5500<\/p>\n<p>JSM-6301F<\/p>\n<p>JSM7600F<\/p>\n<\/td>\n<td style=\"width: 230px; text-align: center;\">\n<p>SEM\u5f62\u8c8c\u89c2\u5bdf<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 230px; text-align: center;\">\n<p>EDS\u70b9\/\u7ebf\u626b<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 230px; text-align: center;\">\n<p>EDS\u9762\u626b<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 230px; text-align: center;\">\n<p>EDS\u5f62\u6001\u5b66\u5206\u6790<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 230px; text-align: center;\">\n<p>EDS\u9897\u7c92\u5206\u6790<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 230px; text-align: center;\">\n<p>EBSD\u632f\u52a8\u629b\u5149<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 230px; text-align: center;\">\n<p>EBSD\u6d4b\u8bd5<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 230px; text-align: center;\">\n<p>\u900f\u5c04\u50cf\uff08\u660e\u573a\u548c\u6697\u573a\uff09<\/p>\n<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p><strong><span style=\"color: #3366ff;\">\u626b\u63cf\u96a7\u9053\u663e\u5fae\u955c-STM<\/span><\/strong><\/p>\n<table style=\"width: 100%;\">\n<tbody>\n<tr>\n<td style=\"width: 183px;\" rowspan=\"2\">\n<p>\u626b\u63cf\u96a7\u9053\u663e\u5fae\u955c<\/p>\n<\/td>\n<td style=\"width: 335px;\" rowspan=\"2\">\n<p>Low-Temperature UHV-STM System<\/p>\n<\/td>\n<td style=\"width: 235px;\">\n<p>\u539f\u5b50\u7ea7\u522b\u9ad8\u5206\u8fa8\u8868\u9762\u5f62\u8c8c\u5206\u6790<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 235px;\">\n<p>\u8868\u9762\u7535\u5b50\u7ed3\u6784\u8868\u5f81<\/p>\n<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p><strong><span style=\"color: #3366ff;\">\u00a0\u7535\u955c\u5236\u6837<\/span><\/strong><\/p>\n<table style=\"width: 100%;\">\n<tbody>\n<tr>\n<td style=\"width: 186px; text-align: center;\" rowspan=\"7\">\n<p>\u805a\u7126\u79bb\u5b50\u675f\uff08\u53cc\u675f\uff09<\/p>\n<\/td>\n<td style=\"width: 324px; text-align: center;\" rowspan=\"7\">\n<p>Auriga FIB<\/p>\n<\/td>\n<td style=\"width: 237px; text-align: center;\">\n<p>\u5f62\u8c8c\u89c2\u5bdf<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 237px; text-align: center;\">\n<p>\u5143\u7d20\u5b9a\u6027\u5b9a\u91cf\u5206\u6790<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 237px; text-align: center;\">\n<p>\u6676\u4f53\u53d6\u5411\u5206\u6790<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 237px; text-align: center;\">\n<p>\u539f\u5b50\u5e8f\u6570\u886c\u5ea6\u50cf<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 237px; text-align: center;\">\n<p>\u79bb\u5b50\u675f\u52a0\u5de5\u4e0e\u6c89\u79ef<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 237px; text-align: center;\">\n<p>\u7eb3\u7c73\u624b\u64cd\u63a7\uff08Omniprobe 200\uff09<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 237px; text-align: center;\">\n<p>3D\u6210\u50cf\uff08\u56fe\u50cf\u3001\u6210\u5206\u3001\u6676\u4f53\u53d6\u5411\uff09<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 186px; text-align: center;\">\n<p>\u79bb\u5b50\u675f\u9540\u819c\u4e0e\u523b\u8680\u7cfb\u7edf<\/p>\n<\/td>\n<td style=\"width: 324px; text-align: center;\">\n<p>Gatan 682<\/p>\n<\/td>\n<td style=\"width: 237px; text-align: center;\">\n<p>\u78b3\u819c\uff08\u6216\u94ec\u3001\u91d1\u3001\u94c2\u7b49\uff09<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 186px; text-align: center;\">\n<p>\u79bb\u5b50\u51cf\u8584\u4eea<\/p>\n<\/td>\n<td style=\"width: 324px; text-align: center;\">\n<p>RES 101<\/p>\n<\/td>\n<td style=\"width: 237px; text-align: center;\">\n<p>\u900f\u5c04\/\u626b\u63cf\u7535\u955c\u6837\u54c1\u7684\u51cf\u8584\uff0c\u6e05\u6d17\u548c\u539f\u4f4d\u55b7\u9540<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 186px; text-align: center;\">\n<p>\u79bb\u5b50\u51cf\u8584\u4eea<\/p>\n<\/td>\n<td style=\"width: 324px; text-align: center;\">\n<p>PIPS \u2161 695<\/p>\n<\/td>\n<td style=\"width: 237px; text-align: center;\">\n<p>\u900f\u5c04\u7535\u955c\u6837\u54c1\u7684\u51cf\u8584\uff0c\u6e05\u6d17<\/p>\n<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p><strong><span style=\"color: #3366ff;\">\u00a0X\u5c04\u7ebf\u884d\u5c04\u4eea<\/span><\/strong><\/p>\n<p>\u6700\u4f4e12K\uff0c\u6700\u9ad81600\u2103\u53d8\u6e29\u6d4b\u8bd5\uff0c\u5e7f\u89d2\u3001\u5c0f\u89d2\u3001\u63a0\u5165\u5c04\u3001\u6b65\u8fdb\u3001\u6162\u626b\u3001\u539f\u4f4d\u3001\u7ec7\u6784\u7b49<\/p>\n<table style=\"width: 100%;\">\n<tbody>\n<tr>\n<td style=\"width: 184px; text-align: center;\" rowspan=\"9\">\n<p>\u539f\u4f4d\u53d8\u6e29X\u5c04\u7ebf\u7c89\u672b\u884d\u5c04\u4eea<\/p>\n<\/td>\n<td style=\"width: 320px; text-align: center;\" rowspan=\"9\">\n<p>\u65e5\u672c\u7406\u5b66D\/max 2550<\/p>\n<p>XRD-7000\u578b<\/p>\n<p>\u5e03\u9c81\u514bD8 Advance<\/p>\n<p>Philips PW 3040\/60\u578b<\/p>\n<p>\u5e15\u7eb3\u79d1 XPert Pro MRD\u9ad8\u5206\u8fa9\u884d\u5c04\u4eea<\/p>\n<\/td>\n<td style=\"width: 245px; text-align: center;\">\n<p>\u4f4e\u6e29XRD\uff0812K\uff09<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 245px; text-align: center;\">\n<p>\u9ad8\u6e29XRD\uff081600\u2103\uff09<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 245px; text-align: center;\">\n<p>\u5c0f\u89d2\u6563\u5c04<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 245px; text-align: center;\">\n<p>\u5c0f\u89d2\u884d\u5c04<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 245px; text-align: center;\">\n<p>\u5e7f\u89d2<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 245px; text-align: center;\">\n<p>\u63a0\u5165\u5c04<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 245px; text-align: center;\">\n<p>\u6162\u626b<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 245px; text-align: center;\">\n<p>\u5e38\u89c4\u5e7f\u89d2<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 245px; text-align: center;\">\n<p>\u7cbe\u4fee\u8ba1\u7b97\u670d\u52a1<\/p>\n<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p><strong><span style=\"color: #3366ff;\">\u7269\u7406\u5438\u9644<\/span><\/strong><\/p>\n<table style=\"width: 100%;\">\n<tbody>\n<tr>\n<td style=\"width: 183px; text-align: center;\" rowspan=\"3\">\n<p>\u6bd4\u8868\u9762\u79ef\u548c\u5b54\u5f84\u5206\u6790\u4eea<\/p>\n<\/td>\n<td style=\"width: 320px; text-align: center;\" rowspan=\"3\">\n<p>\u9ea6\u514bASAP2020<\/p>\n<\/td>\n<td style=\"width: 248px; text-align: center;\">\n<p>BET<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 248px; text-align: center;\">\n<p>\u5fae\u5b54\u5206\u5e03<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 248px; text-align: center;\">\n<p>\u4ecb\u5b54\u5206\u5e03<\/p>\n<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p>\u00a0<strong><span style=\"color: #3366ff;\">\u5316\u5b66\u5438\u9644<\/span><\/strong><\/p>\n<table style=\"width: 100%;\">\n<tbody>\n<tr>\n<td style=\"width: 183px; text-align: center;\" rowspan=\"4\">\n<p>\u5168\u81ea\u52a8\u5316\u5b66\u5438\u9644\u4eea<\/p>\n<\/td>\n<td style=\"width: 319px; text-align: center;\" rowspan=\"4\">\n<p>\u9ea6\u514bAutoChem1 II 2920<\/p>\n<\/td>\n<td style=\"width: 250px; text-align: center;\">\n<p>\u7a0b\u5e8f\u5347\u6e29\u8fd8\u539f\uff08TPR\uff09<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 250px; text-align: center;\">\n<p>\u7a0b\u5e8f\u5347\u6e29\u8131\u9644\uff08TPD\uff09<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 250px; text-align: center;\">\n<p>\u7a0b\u5e8f\u5347\u6e29\u6c27\u5316\uff08TPO\uff09<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 250px; text-align: center;\">\n<p>\u7a0b\u5e8f\u5347\u6e29\u53cd\u5e94\u8bc4\u4ef7<\/p>\n<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p><strong><span style=\"color: #3366ff;\">\u00a0\u7c92\u5ea6\u5206\u5e03<\/span><\/strong><\/p>\n<table style=\"width: 100%;\">\n<tbody>\n<tr>\n<td style=\"width: 184px; text-align: center;\">\n<p>\u6fc0\u5149\u7c92\u5ea6\u5206\u6790\u4eea<\/p>\n<\/td>\n<td style=\"width: 322px; text-align: center;\">\n<p>MS2000<\/p>\n<\/td>\n<td style=\"width: 246px; text-align: center;\">\n<p>\u5fae\u7c73\u7c92\u5ea6\u53ca\u7c92\u5ea6\u5206\u5e03<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 184px; text-align: center;\" rowspan=\"2\">\n<p>\u7eb3\u7c73\u7c92\u5ea6\u53caZeta\u5206\u6790\u4eea<\/p>\n<\/td>\n<td style=\"width: 322px; text-align: center;\" rowspan=\"2\">\n<p>NanoZS+MPT2<\/p>\n<\/td>\n<td style=\"width: 246px; text-align: center;\">\n<p>\u7eb3\u7c73\u7c92\u5ea6\u5206\u5e03\u6d4b\u5b9a<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 246px; text-align: center;\">\n<p>Zeta\u7535\u4f4d<\/p>\n<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p><strong><span style=\"color: #3366ff;\">TG\u3001DSC<\/span><\/strong><\/p>\n<p>\u70ed\u91cd\u3001\u70ed\u7113\u3001\u6bd4\u70ed\u7b49\u6d4b\u8bd5\uff0c<strong>\u53ef\u6d4b-180\u2103\u52301600\u2103\u8303\u56f4\u5185\u5404\u9879\u6570\u636e<\/strong><\/p>\n<table style=\"width: 100%;\">\n<tbody>\n<tr>\n<td style=\"width: 184px;\">\n<p style=\"text-align: center;\">DSC<\/p>\n<\/td>\n<td style=\"width: 312px; text-align: center;\" rowspan=\"4\">\n<p>Netzsch\uff0cSTA449F3<\/p>\n<p>Mettler DSC3<\/p>\n<p>Netzsch\uff0cDSC204F1<\/p>\n<p>Netzsch\/Bruker TG209F3\/Tensor 27<\/p>\n<p>TA Q600<\/p>\n<p>Netzsch\uff0c404 F3<\/p>\n<\/td>\n<td style=\"width: 244px;\">\n<p>\u5e38\u89c4DSC\u6d4b\u8bd5<\/p>\n<p>&nbsp;<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 184px; text-align: center;\">\n<p>TG<\/p>\n<\/td>\n<td style=\"width: 244px; text-align: center;\">\n<p>TG-DSC\u6d4b\u8bd5<\/p>\n<p>&nbsp;<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 184px; text-align: center;\">\n<p>TG-DSC<\/p>\n<\/td>\n<td style=\"width: 244px; text-align: center;\">\n<p>\u6c27\u5316\u8bf1\u5bfc\u671f<\/p>\n<p>&nbsp;<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 184px; text-align: center;\">\n<p>TG-IR<\/p>\n<\/td>\n<td style=\"width: 244px; text-align: center;\">\n<p>\u6bd4\u70ed<\/p>\n<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p><strong><span style=\"color: #3366ff;\">\u5bfc\u70ed<\/span><\/strong><\/p>\n<p>\u6d4b\u70ed\u5bfc\u7387\u6700\u4f4e\u6e29\u5ea6\u53ef\u6d4b\u52304.2K\uff0c\u6700\u9ad8\u6d4b\u52301100\u2103\uff0c100\u2103\u4ee5\u4e0b\u53ef\u76f4\u63a5\u6d4b\u51fa\uff0c100\u2103\u4ee5\u4e0a\u9700\u8981\u901a\u8fc7\u6d4b\u70ed\u6269\u6563\u7cfb\u6570\u548c\u6bd4\u70ed\u540e\u8ba1\u7b97<\/p>\n<table style=\"width: 100%;\">\n<tbody>\n<tr>\n<td style=\"width: 188px; text-align: center;\">\n<p>\u6fc0\u5149\u5bfc\u70ed\u4eea\uff08LFA457\uff09<\/p>\n<\/td>\n<td style=\"width: 311px; text-align: center;\" rowspan=\"5\">\n<p>LFA457<\/p>\n<p>LFA447<\/p>\n<p>NETZSCH\uff0c LFA-457<\/p>\n<\/td>\n<td style=\"width: 243px; text-align: center;\" rowspan=\"2\">\n<p>\u70ed\u6269\u6563\u7cfb\u6570<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 188px; text-align: center;\">\n<p>\u6fc0\u5149\u5bfc\u70ed\u4eea\uff08LFA447\uff09<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 188px; text-align: center;\">\n<p>\u6fc0\u5149\u70ed\u5bfc\u4eea<\/p>\n<\/td>\n<td style=\"width: 243px; text-align: center;\">\n<p>\u70ed\u6269\u6563\u7cfb\u6570<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 188px; text-align: center;\">\n<p>\u5bfc\u70ed\u6d4b\u8bd5\u4eea<\/p>\n<\/td>\n<td style=\"width: 243px; text-align: center;\">\n<p>\u5bfc\u70ed\u7cfb\u6570<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 188px; text-align: center;\">\n<p>\u6bd4\u70ed\u6d4b\u8bd5\u4eea<\/p>\n<\/td>\n<td style=\"width: 243px; text-align: center;\">\n<p>\u5ba4\u6e29-4.2K<\/p>\n<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p><strong><span style=\"color: #3366ff;\">\u52a8\u6001\u70ed\u673a\u68b0\u5206\u6790-DMA<\/span><\/strong><\/p>\n<table style=\"width: 100%;\">\n<tbody>\n<tr>\n<td style=\"width: 189px;\">\n<p>\u52a8\u6001\u70ed\u673a\u68b0\u5206\u6790\u4eea<\/p>\n<\/td>\n<td style=\"width: 311px;\">\n<p>\uff08Netzsch\uff09DMA242E<\/p>\n<\/td>\n<td style=\"width: 244px;\">\n<p>\u5ba4\u6e29\uff5e600\u2103<\/p>\n<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p><strong><span style=\"color: #3366ff;\">\u5085\u91cc\u53f6\u7ea2\u5916<\/span><\/strong><\/p>\n<p>\u53ef\u6d4b\u666e\u901a\u7ea2\u5916\u3001ATR\u7ea2\u5916\u3001\u539f\u4f4d\u7ea2\u5916\u548c\u5421\u5576\u7ea2\u5916\u7b49\uff0c\u5728\u5ba4\u6e29\u5230900\u2103\u6e29\u533a\u5185\u63d0\u4f9b\u591a\u79cd\u6c14\u6c1b<\/p>\n<table style=\"width: 100%;\">\n<tbody>\n<tr>\n<td style=\"width: 183px; text-align: center;\">\n<p>\u5085\u7acb\u53f6\u53d8\u6362\u7ea2\u5916\u5149\u8c31\u4eea\uff08\u5e26\u539f\u4f4d\u53cd\u5e94\u6c60\uff09<\/p>\n<\/td>\n<td style=\"width: 310px; text-align: center;\">\n<p>Nicolet is50<\/p>\n<p>Thermo fisher Nicolet 6700<\/p>\n<p>Bruker Tensor 27<\/p>\n<\/td>\n<td style=\"width: 250px; text-align: center;\">\n<p>\u8870\u51cf\u5168\u53cd\u5c04ATR<\/p>\n<p>\u900f\u5c04\u7ea2\u5916 KBr\u538b\u7247<\/p>\n<p>\u900f\u5c04\u7ea2\u5916 \u65e0\u9700KBr\u538b\u7247<\/p>\n<p>\u6f2b\u53cd\u5c04<\/p>\n<p>\u539f\u4f4d\u7ea2\u5916<\/p>\n<p>\u5421\u5576\u7ea2\u5916<\/p>\n<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p>X\u5c04\u7ebf\u5149\u7535\u5b50\u80fd\u8c31\u4eea XPS<\/p>\n<table style=\"width: 100%;\">\n<tbody>\n<tr>\n<td style=\"width: 179px; text-align: center;\" rowspan=\"12\">\n<p>X\u5c04\u7ebf\u5149\u7535\u5b50\u80fd\u8c31\u4eea<\/p>\n<\/td>\n<td style=\"width: 311px; text-align: center;\" rowspan=\"12\">\n<p>PHI 5000 Versaprobe II<\/p>\n<p>Kratos Axis Ultra DLD<\/p>\n<p>Thermo Scientific ESCALAB 250Xi<\/p>\n<\/td>\n<td style=\"width: 244px; text-align: center;\">\n<p>\u5e38\u89c4\u5bbd\u8c31\u626b\u63cf<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 244px; text-align: center;\">\n<p>\u7a84\u8c31\u626b\u63cf<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 244px; text-align: center;\">\n<p>\u7d2b\u5916\u5149\u7535\u5b50\u80fd\u8c31\uff08UPS\uff09<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 244px; text-align: center;\">\n<p>\u9009\u533a\u6210\u50cf mapping<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 244px; text-align: center;\">\n<p>Ar\u79bb\u5b50\u523b\u8680\uff08\u4e0d\u542b\u91c7\u8c31\uff09<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 244px; text-align: center;\">\n<p>Ar\u56e2\u7c07\u79bb\u5b50\u6df1\u5ea6\u5256\u6790\uff08\u91c7\u8c31\u53e6\u8ba1\uff09<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 244px; text-align: center;\">\n<p>Al\/Mg\u53cc\u9633\u6781<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 244px; text-align: center;\">\n<p>\u539f\u4f4d\u9ad8\u4f4e\u6e29\uff08153~773K\uff09<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 244px; text-align: center;\">\n<p>\u51c6\u539f\u4f4d\u9ad8\u4f4e\u6e29\uff08123~1073K\uff09<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 244px; text-align: center;\">\n<p>\u89d2\u5206\u8fa8XPS<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 244px; text-align: center;\">\n<p>AES\uff08\u4fc4\u6b47\u80fd\u8c31\uff09<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 244px; text-align: center;\">\n<p>REELS\u3001ISS<\/p>\n<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p><strong><span style=\"color: #3366ff;\">\u5143\u7d20\u5206\u6790<\/span><\/strong><\/p>\n<p>\u53ef\u4ee5\u5206\u6790\u5404\u79cd\u65e0\u673a\u6837\u54c1\u3001\u6709\u673a\u6837\u54c1\u3001\u91d1\u5c5e\u6837\u54c1\u5143\u7d20\u542b\u91cf\uff0c\u5206\u679092\u53f7\u4ee5\u524d\u7684\u5168\u90e8\u5143\u7d20\u3002<\/p>\n<table style=\"width: 100%;\">\n<tbody>\n<tr>\n<td style=\"width: 185px; text-align: center;\" rowspan=\"2\">\n<p>CHNSO\u6709\u673a\u5143\u7d20\u5206\u6790\u4eea<\/p>\n<\/td>\n<td style=\"width: 300px; text-align: center;\">\n<p>Vario el cube<\/p>\n<\/td>\n<td style=\"width: 253px; text-align: center;\" rowspan=\"2\">\n<p>CHNS\u5143\u7d20<\/p>\n<p>O\u5143\u7d20<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 300px; text-align: center;\">\n<p>\u5fb7\u56fdElementar\u516c\u53f8Vario EL \u2162<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 185px; text-align: center;\">\n<p>\u7535\u611f\u8026\u5408\u7b49\u79bb\u5b50\u539f\u5b50\u53d1\u5c04\u5149\u8c31\u4eea<\/p>\n<\/td>\n<td style=\"width: 300px; text-align: center;\">\n<p>Thermo iCAP-6000<\/p>\n<p>OPTIMA 8000DV<\/p>\n<\/td>\n<td style=\"width: 253px; text-align: center;\">\n<p>\u5143\u7d20\u542b\u91cf<\/p>\n<p>\u5168\u5143\u7d20\u5b9a\u91cf\uff08\u540c\u65f6\u6d4b\u5b9a55\u79cd\u5143\u7d20\uff09<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 185px; text-align: center;\" rowspan=\"3\">\n<p>X\u5c04\u7ebf\u8367\u5149\u5149\u8c31\u4eea\uff08XRF\uff09<\/p>\n<\/td>\n<td style=\"width: 300px; text-align: center;\" rowspan=\"3\">\n<p>\u5c9b\u6d25XRF-1800\u578b \u6ce2\u957f\u8272\u6563\u8367\u5149\u5149\u8c31\u4eea<\/p>\n<\/td>\n<td style=\"width: 253px; text-align: center;\">\n<p>\u5b9a\u6027<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 253px; text-align: center;\">\n<p>\u5b9a\u91cf<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 253px; text-align: center;\">\n<p>\u5168\u5143\u7d20\u5b9a\u91cf<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 185px; text-align: center;\">\n<p>\u7ea2\u5916\u78b3\u786b\u4eea<\/p>\n<\/td>\n<td style=\"width: 300px; text-align: center;\">\n<p>\u529b\u53efCS344<\/p>\n<\/td>\n<td style=\"width: 253px; text-align: center;\">\n<p>C\u3001S\u542b\u91cf<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 185px; text-align: center;\">\n<p>\u7ea2\u5916\u6c2e\u6c27\u4eea<\/p>\n<\/td>\n<td style=\"width: 300px; text-align: center;\">\n<p>\u529b\u53efTC400<\/p>\n<\/td>\n<td style=\"width: 253px; text-align: center;\">\n<p>N\u3001O\u542b\u91cf<\/p>\n<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p>\u00a0<strong><span style=\"color: #3366ff;\">\u539f\u4f4d\u62c9\u66fc\u5149\u8c31<\/span><\/strong><\/p>\n<p>\u6d4b\u6e29\u8303\u56f4\uff1a80-473K\uff0c325\u00a0514\u00a0532\u00a0633\u00a0780nm\u00a0\u6ce2\u957f\u90fd\u6709<\/p>\n<table style=\"width: 100%;\">\n<tbody>\n<tr>\n<td style=\"width: 187px; text-align: center;\">\n<p>\u62c9\u66fc\u5149\u8c31\u4eea<\/p>\n<p>\u5171\u7126\u663e\u5fae\u62c9\u66fc\u5149\u8c31\u4eea<\/p>\n<\/td>\n<td style=\"width: 302px; text-align: center;\">\n<p>LabRAMHR 800<\/p>\n<p>\u96f7\u5c3c\u7ecdRiVia<\/p>\n<\/td>\n<td style=\"width: 248px; text-align: center;\">\n<p>\u666e\u901a\u626b\u8c31\uff08325nm \uff09<\/p>\n<p>\u666e\u901a\u626b\u8c31\uff08532nm\u3001785nm\u3001633nm\uff09<\/p>\n<p>\u9ad8\u4f4e\u6e29\u6d4b\u8bd5(LINKAM)<\/p>\n<p>\u539f\u4f4d\u62c9\u66fc\u5149\u8c31\u6d4b\u8bd5\uff08mapping+\u7535\u5316\u5b66\u5de5\u4f5c\u7ad9\uff09<\/p>\n<p>\u5927\u5149\u6591\u626b\u63cf\uff08DUOSCAN\uff09<\/p>\n<p>\u53d8\u6e29\u6d4b\u8bd5\uff0880-473K\uff09<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 187px; text-align: center;\">\n<p>\u7d2b\u5916\u53ef\u89c1\u8fd1\u7ea2\u5916\u5206\u5149\u5149\u5ea6\u8ba1<\/p>\n<\/td>\n<td style=\"width: 302px; text-align: center;\">\n<p>Cary 5000<\/p>\n<p>\u5c9b\u6d25UV360<\/p>\n<\/td>\n<td style=\"width: 248px; text-align: center;\">\n<p>\u7d2b\u5916\u53ef\u89c1\u8fd1\u7ea2\u5916\u5149\u8c31<\/p>\n<p>\u6db2\u4f53\u6837\u54c1\u7d2b\u5916\u5438\u6536\u6d4b\u8bd5<\/p>\n<p>\u56fa\u4f53\u6837\u54c1\u900f\u8fc7\u7387<\/p>\n<p>\u53cd\u5c04\u7387\u6d4b\u8bd5<\/p>\n<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p>\u00a0<strong><span style=\"color: #3366ff;\">\u6781\u4f4e\u6e29\u529b\u5b66\u6027\u80fd<\/span><\/strong><\/p>\n<p>\u53ef\u6d4b\u6750\u6599\u5728\u6db2\u6c26\u3001\u6db2\u6c2e\u4ee5\u53ca\u5e38\u6e29\u4e0b\u7684\u529b\u5b66\u6027\u80fd<\/p>\n<table style=\"width: 100%;\">\n<tbody>\n<tr>\n<td style=\"width: 181px; text-align: center;\" colspan=\"2\" rowspan=\"23\">\n<p>\u7535\u5b50\u4e07\u80fd\u6750\u6599\u8bd5\u9a8c\u673a<\/p>\n<p>\uff08\u591a\u53f0\u3001\u8f7d\u8377\u7b49\u53c2\u6570\u4e0d\u540c\uff09<\/p>\n<\/td>\n<td style=\"width: 299px; text-align: center;\" rowspan=\"4\">\n<p>\u62c9\u4f38\u5f3a\u5ea6<\/p>\n<\/td>\n<td style=\"width: 251px; text-align: center;\">\n<p>\u5ba4\u6e29<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 251px; text-align: center;\">\n<p>\u6db2\u6c2e<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 251px; text-align: center;\">\n<p>20K<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 251px; text-align: center;\">\n<p>4.2K<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 299px; text-align: center;\" rowspan=\"4\">\n<p>\u5f2f\u66f2\u5f3a\u5ea6<\/p>\n<\/td>\n<td style=\"width: 251px; text-align: center;\">\n<p>\u5ba4\u6e29<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 251px; text-align: center;\">\n<p>\u6db2\u6c2e<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 251px; text-align: center;\">\n<p>20K<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 251px; text-align: center;\">\n<p>4.2K<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 299px; text-align: center;\" rowspan=\"3\">\n<p>\u65ad\u88c2\u97e7\u6027<\/p>\n<\/td>\n<td style=\"width: 251px; text-align: center;\">\n<p>\u5ba4\u6e29<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 251px; text-align: center;\">\n<p>\u6db2\u6c2e<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 251px; text-align: center;\">\n<p>\u6db2\u6c26<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 299px; text-align: center;\" rowspan=\"4\">\n<p>\u538b\u7f29\u5f3a\u5ea6<\/p>\n<\/td>\n<td style=\"width: 251px; text-align: center;\">\n<p>\u5ba4\u6e29<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 251px; text-align: center;\">\n<p>\u6db2\u6c2e<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 251px; text-align: center;\">\n<p>20K<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 251px; text-align: center;\">\n<p>4.2K<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 299px; text-align: center;\" rowspan=\"4\">\n<p>\u51b2\u51fb\u97e7\u6027<\/p>\n<\/td>\n<td style=\"width: 251px; text-align: center;\">\n<p>\u5ba4\u6e29<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 251px; text-align: center;\">\n<p>\u6db2\u6c2e<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 251px; text-align: center;\">\n<p>20K<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 251px; text-align: center;\">\n<p>4.2K<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 299px; text-align: center;\" rowspan=\"4\">\n<p>\u526a\u5207\u5f3a\u5ea6<\/p>\n<\/td>\n<td style=\"width: 251px; text-align: center;\">\n<p>\u5ba4\u6e29<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 251px; text-align: center;\">\n<p>\u6db2\u6c2e<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 251px; text-align: center;\">\n<p>20K<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 251px; text-align: center;\">\n<p>4.2K<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 71px; text-align: center;\">\n<p>\u5fae\u673a\u63a7\u4e07\u80fd\u8bd5\u9a8c\u673a<\/p>\n<\/td>\n<td style=\"width: 110px; text-align: center;\">\n<p>CMT6104<\/p>\n<\/td>\n<td style=\"width: 299px; text-align: center;\">\n<p>\u4e09\u89d2\u5f2f\u66f2\u53d8\u5f62\u3001\u8584\u819c\u62c9\u4f38\u3001\u62c9\u4f38\u5f3a\u5ea6<\/p>\n<\/td>\n<td style=\"width: 251px; text-align: center;\">\u00a0<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 71px; text-align: center;\" rowspan=\"2\">\n<p>\u5168\u81ea\u52a8\u7535\u5b50\u4e07\u80fd\u6750\u6599\u8bd5\u9a8c\u673a<\/p>\n<\/td>\n<td style=\"width: 110px; text-align: center;\" rowspan=\"2\">\n<p>Zwick Z100<\/p>\n<p>Zwick Z050<\/p>\n<\/td>\n<td style=\"width: 299px; text-align: center;\" rowspan=\"2\">\n<p>\u62c9\u4f38<\/p>\n<\/td>\n<td style=\"width: 251px; text-align: center;\">\n<p>\u5e38\u6e29<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 251px; text-align: center;\">\n<p>100-400\u2103<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 71px; text-align: center;\" rowspan=\"5\">\n<p>\u51b2\u51fb\u8bd5\u9a8c\u673a<\/p>\n<\/td>\n<td style=\"width: 110px; text-align: center;\" rowspan=\"5\">\n<p>\u4e09\u601d\u7eb5\u6a2a300J<\/p>\n<p>MTS-SANS<\/p>\n<p>ZBC-300A<\/p>\n<p>PMT-1200<\/p>\n<\/td>\n<td style=\"width: 299px; text-align: center;\" rowspan=\"5\">\n<p>\u51b2\u51fb\u97e7\u6027<\/p>\n<\/td>\n<td style=\"width: 251px; text-align: center;\">\n<p>\u5ba4\u6e29<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 251px; text-align: center;\">\n<p>\u5ba4\u6e29<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 251px; text-align: center;\">\n<p>\u6db2\u6c2e<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 251px; text-align: center;\">\n<p>20K<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 251px; text-align: center;\">\n<p>4.2K<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 71px; text-align: center;\" rowspan=\"3\">\n<p>\u75b2\u52b3\u8bd5\u9a8c\u673a<\/p>\n<\/td>\n<td style=\"width: 110px; text-align: center;\" rowspan=\"3\">\n<p>PLS100<\/p>\n<p>Instron 8802<\/p>\n<\/td>\n<td style=\"width: 299px; text-align: center;\" rowspan=\"3\">\n<p>\u75b2\u52b3<\/p>\n<\/td>\n<td style=\"width: 251px; text-align: center;\">\n<p>\u5ba4\u6e29<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 251px; text-align: center;\">\n<p>\u6db2\u6c26<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 251px; text-align: center;\">\n<p>\u6db2\u6c2e<\/p>\n<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p><strong><span style=\"color: #3366ff;\">\u00a0\u786c\u5ea6<\/span><\/strong><\/p>\n<table style=\"width: 100%;\">\n<tbody>\n<tr>\n<td style=\"width: 183px; text-align: center;\">\n<p>\u6570\u663e\u5e03\u6d1b\u7ef4\u786c\u5ea6\u8ba1<\/p>\n<\/td>\n<td style=\"width: 300px; text-align: center;\">\n<p>SHBRV-187.5<\/p>\n<\/td>\n<td style=\"width: 249px; text-align: center;\">\n<p>\u786c\u5ea6\u6d4b\u8bd5<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 183px; text-align: center;\">\n<p>\u663e\u5fae\u7ef4\u5f0f\u786c\u5ea6\u8ba1<\/p>\n<\/td>\n<td style=\"width: 300px; text-align: center;\">\n<p>EM-1500L<\/p>\n<\/td>\n<td style=\"width: 249px; text-align: center;\">\n<p>\u7ef4\u5f0f\u786c\u5ea6\u6d4b\u8bd5<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 183px; text-align: center;\">\n<p>\u5e03\u6c0f\u786c\u5ea6\u8ba1<\/p>\n<\/td>\n<td style=\"width: 300px; text-align: center;\">\n<p>MHB-3000<\/p>\n<\/td>\n<td style=\"width: 249px; text-align: center;\" rowspan=\"3\">\n<p>\u786c\u5ea6<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 183px; text-align: center;\">\n<p>\u6d1b\u6c0f\u786c\u5ea6\u8ba1<\/p>\n<\/td>\n<td style=\"width: 300px; text-align: center;\">\n<p>HRS-150<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 183px; text-align: center;\">\n<p>\u7ef4\u6c0f\u786c\u5ea6\u8ba1<\/p>\n<\/td>\n<td style=\"width: 300px; text-align: center;\">\n<p>HVS-30P<\/p>\n<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p><strong><span style=\"color: #3366ff;\">\u7ebf\u81a8\u80c0\u6d4b\u8bd5\uff08\u8d85\u5927\u6e29\u5ea6\u8303\u56f4\uff09<\/span><\/strong><\/p>\n<p>\u6700\u4f4e\u6e29\u5ea6\u53ef\u8fbe4.2K\uff0c\u6700\u9ad8\u6e29\u5ea6\u80fd\u52302800\u2103\u3002<\/p>\n<table style=\"width: 100%;\">\n<tbody>\n<tr>\n<td style=\"width: 186px; text-align: center;\">\n<p>\u7ebf\u81a8\u80c0\u6d4b\u8bd5\u4eea<\/p>\n<\/td>\n<td style=\"width: 296px; text-align: center;\">\n<p>\u5fb7\u56fdLinseis\uff0cL75<\/p>\n<p>\u8010\u9a70 DIL402C<\/p>\n<\/td>\n<td style=\"width: 255px; text-align: center;\">\n<p>\u7ebf\u81a8\u80c0\u7cfb\u6570<\/p>\n<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p><strong><span style=\"color: #3366ff;\">\u00a0\u7535\u6c60\u6d4b\u8bd5\u8bbe\u5907<\/span><\/strong><\/p>\n<table style=\"width: 100%;\">\n<tbody>\n<tr>\n<td style=\"width: 184px; text-align: center;\">\n<p>\u7814\u7a76\u578b\u63a5\u89e6\u89d2\u6d4b\u91cf\u4eea<\/p>\n<\/td>\n<td style=\"width: 296px; text-align: center;\">\n<p>DSA30<\/p>\n<\/td>\n<td style=\"width: 256px; text-align: center;\">\n<p>\u63a5\u89e6\u89d2<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 184px; text-align: center;\">\n<p>\u8868\u9762\u5f20\u529b\u6d4b\u8bd5\u4eea<\/p>\n<\/td>\n<td style=\"width: 296px; text-align: center;\">\n<p>&nbsp;<\/p>\n<\/td>\n<td style=\"width: 256px; text-align: center;\">\n<p>\u8868\u9762\u5f20\u529b<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 184px; text-align: center;\" rowspan=\"2\">\n<p>\u6c34\u5206\u6d4b\u5b9a\u4eea<\/p>\n<\/td>\n<td style=\"width: 296px; text-align: center;\" rowspan=\"2\">\n<p>831 KF<\/p>\n<\/td>\n<td style=\"width: 256px; text-align: center;\">\n<p>\u56fa\u4f53\u6c34\u5206\u6d4b\u5b9a<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>\u6db2\u4f53\u6c34\u5206\u6d4b\u5b9a<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 184px; text-align: center;\">\n<p>\u5168\u81ea\u52a8\u771f\u5bc6\u5ea6\u5206\u6790\u4eea<\/p>\n<\/td>\n<td style=\"width: 296px; text-align: center;\">\n<p>AccuPyc II 1340<\/p>\n<\/td>\n<td style=\"width: 256px; text-align: center;\">\n<p>\u771f\u5bc6\u5ea6<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 184px; text-align: center;\">\n<p>\u5168\u81ea\u52a8\u632f\u5b9e\u5bc6\u5ea6\u5206\u6790\u4eea<\/p>\n<\/td>\n<td style=\"width: 296px; text-align: center;\">\n<p>GeoPyc 1360<\/p>\n<\/td>\n<td style=\"width: 256px; text-align: center;\">\n<p>\u632f\u5b9e\u5bc6\u5ea6<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 184px; text-align: center;\">\n<p>\u624b\u5957\u7bb1<\/p>\n<\/td>\n<td style=\"width: 296px; text-align: center;\">\n<p>M.BRUN\u53cc\u5de5\u4f4d<\/p>\n<\/td>\n<td style=\"width: 256px; text-align: center;\">\n<p>\u624b\u5957\u7bb1\u673a\u65f6<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 184px; text-align: center;\" rowspan=\"2\">\n<p>\u7535\u5316\u5b66\u5de5\u4f5c\u7ad9\uff08VMP3\uff09<\/p>\n<\/td>\n<td style=\"width: 296px; text-align: center;\" rowspan=\"2\">\n<p>VMP3<\/p>\n<\/td>\n<td style=\"width: 256px; text-align: center;\">\n<p>EIS<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>CV \u3001\u5145\u653e\u7535\u7b49<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 184px; text-align: center;\" rowspan=\"2\">\n<p>\u7535\u5316\u5b66\u5de5\u4f5c\u7ad9\uff08Solartron\uff09<\/p>\n<\/td>\n<td style=\"width: 296px; text-align: center;\" rowspan=\"2\">\n<p>Solartron 1470E<\/p>\n<\/td>\n<td style=\"width: 256px; text-align: center;\">\n<p>EIS<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>CV \u3001\u5145\u653e\u7535\u7b49<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 184px; text-align: center;\">\n<p>\u84dd\u7535\u6d4b\u8bd5\u4eea<\/p>\n<\/td>\n<td style=\"width: 296px; text-align: center;\">\n<p>CT 2001A<\/p>\n<\/td>\n<td style=\"width: 256px; text-align: center;\">\n<p>\u6052\u6d41\/\u6052\u538b\u5145\u653e\u7535<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 184px; text-align: center;\" rowspan=\"5\">\n<p>\u52a8\u529b\u7535\u6c60<br \/>\n \u6d4b\u8bd5\u4eea<\/p>\n<\/td>\n<td style=\"width: 296px; text-align: center;\" rowspan=\"5\">\n<p>S4000<\/p>\n<\/td>\n<td style=\"width: 256px; text-align: center;\">\n<p>\u7535\u6027\u80fd\u6d4b\u8bd5\u00a0 \u00a0\u226415A\u91cf\u7a0b<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>\u7535\u6027\u80fd\u6d4b\u8bd5\u00a0\u00a0 100A\u91cf\u7a0b<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>\u7535\u6027\u80fd\u6d4b\u8bd5\u00a0\u00a0 200A\u91cf\u7a0b<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>\u7535\u6027\u80fd\u6d4b\u8bd5\u00a0\u00a0 400A\u91cf\u7a0b<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>\u7535\u6027\u80fd\u6d4b\u8bd5 \u00a0\u00a0800A\u91cf\u7a0b<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 184px; text-align: center;\" rowspan=\"3\">\n<p>\u632f\u52a8\u8bd5\u9a8c\u673a<\/p>\n<\/td>\n<td style=\"width: 296px; text-align: center;\" rowspan=\"3\">\n<p>DC-300<\/p>\n<\/td>\n<td style=\"width: 256px; text-align: center;\">\n<p>\u22645Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>5-10\uff08\u5305\u542b\uff09Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>10-20\uff08\u5305\u542b\uff09Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 184px; text-align: center;\" rowspan=\"3\">\n<p>\u673a\u68b0\u51b2\u51fb\u8bd5\u9a8c\u673a<\/p>\n<\/td>\n<td style=\"width: 296px; text-align: center;\" rowspan=\"3\">\n<p>CL-50<\/p>\n<\/td>\n<td style=\"width: 256px; text-align: center;\">\n<p>\u22645Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>5-10\uff08\u5305\u542b\uff09Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>10-20\uff08\u5305\u542b\uff09Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 184px; text-align: center;\" rowspan=\"3\">\n<p>\u7535\u6c60\u9ad8\u6e29\u9694\u7206\u8bd5\u9a8c\u673a<\/p>\n<\/td>\n<td style=\"width: 296px; text-align: center;\" rowspan=\"3\">\n<p>DMS-9987<\/p>\n<\/td>\n<td style=\"width: 256px; text-align: center;\">\n<p>\u22645Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>5-10\uff08\u5305\u542b\uff09Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>10-20\uff08\u5305\u542b\uff09Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 184px; text-align: center;\" rowspan=\"3\">\n<p>\u6e29\u63a7\u578b\u7535\u6c60\u77ed\u8def\u8bd5\u9a8c\u673a<\/p>\n<\/td>\n<td style=\"width: 296px; text-align: center;\" rowspan=\"3\">\n<p>DMS-WDL<\/p>\n<\/td>\n<td style=\"width: 256px; text-align: center;\">\n<p>\u22645Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>5-10\uff08\u5305\u542b\uff09Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>10-20\uff08\u5305\u542b\uff09Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 184px; text-align: center;\" rowspan=\"3\">\n<p>\u7535\u6c60\u4f4e\u6c14\u538b\u6a21\u62df\u8bd5\u9a8c\u673a<\/p>\n<\/td>\n<td style=\"width: 296px; text-align: center;\" rowspan=\"3\">\n<p>DMS-9988<\/p>\n<\/td>\n<td style=\"width: 256px; text-align: center;\">\n<p>\u22645Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>5-10\uff08\u5305\u542b\uff09Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>10-20\uff08\u5305\u542b\uff09Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 184px; text-align: center;\" rowspan=\"3\">\n<p>\u7535\u6c60\u81ea\u7531\u8dcc\u843d\u8bd5\u9a8c\u673a<\/p>\n<\/td>\n<td style=\"width: 296px; text-align: center;\" rowspan=\"3\">\n<p>DMS-9985<\/p>\n<\/td>\n<td style=\"width: 256px; text-align: center;\">\n<p>\u22645Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>5-10\uff08\u5305\u542b\uff09Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>10-20\uff08\u5305\u542b\uff09Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 184px; text-align: center;\" rowspan=\"3\">\n<p>\u7535\u6c60\u6324\u538b\u8bd5\u9a8c\u673a<\/p>\n<\/td>\n<td style=\"width: 296px; text-align: center;\" rowspan=\"3\">\n<p>DMS-9981<\/p>\n<\/td>\n<td style=\"width: 256px; text-align: center;\">\n<p>\u22645Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>5-10\uff08\u5305\u542b\uff09Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>10-20\uff08\u5305\u542b\uff09Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 184px; text-align: center;\" rowspan=\"3\">\n<p>\u7535\u6c60\u91cd\u7269\u51b2\u51fb\u8bd5\u9a8c\u673a<\/p>\n<\/td>\n<td style=\"width: 296px; text-align: center;\" rowspan=\"3\">\n<p>DMS-Z9983<\/p>\n<\/td>\n<td style=\"width: 256px; text-align: center;\">\n<p>\u22645Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>5-10\uff08\u5305\u542b\uff09Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>10-20\uff08\u5305\u542b\uff09Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 184px; text-align: center;\" rowspan=\"3\">\n<p>\u7535\u6c60\u71c3\u70e7\u629b\u5c04\u8bd5\u9a8c\u673a<\/p>\n<\/td>\n<td style=\"width: 296px; text-align: center;\" rowspan=\"3\">\n<p>DMS-9986<\/p>\n<\/td>\n<td style=\"width: 256px; text-align: center;\">\n<p>\u22645Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>5-10\uff08\u5305\u542b\uff09Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>10-20\uff08\u5305\u542b\uff09Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 184px; text-align: center;\" rowspan=\"3\">\n<p>\u7535\u6c60\u6d17\u6da4\u8bd5\u9a8c\u673a<\/p>\n<\/td>\n<td style=\"width: 296px; text-align: center;\" rowspan=\"3\">\n<p>DMS-XD<\/p>\n<\/td>\n<td style=\"width: 256px; text-align: center;\">\n<p>\u22645Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>5-10\uff08\u5305\u542b\uff09Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>10-20\uff08\u5305\u542b\uff09Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 184px; text-align: center;\" rowspan=\"3\">\n<p>\u7535\u6c60\u9488\u523a\u8bd5\u9a8c\u673a<\/p>\n<\/td>\n<td style=\"width: 296px; text-align: center;\" rowspan=\"3\">\n<p>DMS-9982<\/p>\n<\/td>\n<td style=\"width: 256px; text-align: center;\">\n<p>\u22645Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>5-10\uff08\u5305\u542b\uff09Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>10-20\uff08\u5305\u542b\uff09Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 184px; text-align: center;\" rowspan=\"3\">\n<p>\u9759\u7535\u653e\u7535\u6a21\u62df\u5668<\/p>\n<\/td>\n<td style=\"width: 296px; text-align: center;\" rowspan=\"3\">\n<p>ESS-B3011\/GT-30R<\/p>\n<\/td>\n<td style=\"width: 256px; text-align: center;\">\n<p>\u22645Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>5-10\uff08\u5305\u542b\uff09Ah<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 256px; text-align: center;\">\n<p>10-20\uff08\u5305\u542b\uff09Ah<\/p>\n<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p><strong><span style=\"color: #3366ff;\">\u00a0\u70ed\u7535<\/span><\/strong><\/p>\n<table style=\"width: 100%;\">\n<tbody>\n<tr>\n<td style=\"width: 180px; text-align: center;\">\n<p>\u70ed\u7535\u6d4b\u8bd5\u7cfb\u7edf<\/p>\n<\/td>\n<td style=\"width: 301px; text-align: center;\">\n<p>Linseis\uff0c LSR-3<\/p>\n<\/td>\n<td style=\"width: 256px; text-align: center;\">\n<p>\u7535\u963b\u7387 Seebeck\u7cfb\u6570<\/p>\n<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p>\u00a0<strong><span style=\"color: #3366ff;\">\u7efc\u5408\u7269\u6027\u6d4b\u91cf\u7cfb\u7edf<\/span><\/strong><\/p>\n<p>\u78c1\u573a\u53ef\u523014T\uff0c\u6e29\u5ea6\u6700\u4f4e\u53ef\u8fbe50mK<\/p>\n<table style=\"width: 100%;\">\n<tbody>\n<tr>\n<td style=\"width: 179px; text-align: center;\">\n<p>PPMS<\/p>\n<\/td>\n<td style=\"width: 298px; text-align: center;\">\n<p>Quantum Design\uff0c<\/p>\n<\/td>\n<td style=\"width: 256px; text-align: center;\">\n<p>\u6750\u6599\u7269\u6027\u6d4b\u8bd5<\/p>\n<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p><strong><span style=\"color: #3366ff;\">\u00a0\u8272\u8c31<\/span><\/strong><\/p>\n<table style=\"width: 100%;\">\n<tbody>\n<tr>\n<td style=\"width: 174px; text-align: center;\">\n<p>\u51dd\u80f6\u6e17\u900f\u8272\u8c31\u4eea<\/p>\n<\/td>\n<td style=\"width: 301px; text-align: center;\">\n<p>Waters E2695<\/p>\n<\/td>\n<td style=\"width: 252px; text-align: center;\">\n<p>\u56db\u6c22\u544b\u5583\u00a0 \u6d4b\u8bd5\u6e29\u5ea6\uff1a30\u00b0C<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 174px; text-align: center;\">\n<p>\u9ad8\u6e29\u51dd\u80f6\u6e17\u900f\u8272\u8c31\u4eea<\/p>\n<\/td>\n<td style=\"width: 301px; text-align: center;\">\n<p>PL-GPC 220<\/p>\n<\/td>\n<td style=\"width: 252px; text-align: center;\">\n<p>\u4e09\u6c2f\u82ef\u00a0 \u6d4b\u8bd5\u6e29\u5ea6\uff1a150\u00b0C<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 174px; text-align: center;\">\n<p>\u5706\u504f\u632f\u8367\u5149\u5149\u8c31\u4eea<\/p>\n<\/td>\n<td style=\"width: 301px; text-align: center;\">\n<p>JASCO CPL-300<\/p>\n<\/td>\n<td style=\"width: 252px; text-align: center;\">\n<p>CPL<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 174px; text-align: center;\">\n<p>\u6c14\u76f8\u8272\u8c31\u8d28\u8c31\u8054\u7528\u4eea\uff08GCMS\uff09<\/p>\n<\/td>\n<td style=\"width: 301px; text-align: center;\">\n<p>Trace1300 ISQ<\/p>\n<\/td>\n<td style=\"width: 252px; text-align: center;\">\n<p>\u6c14\u76f8\u8272\u8c31 \u8d28\u8c31<\/p>\n<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p>\u00a0\u5176\u4ed6<\/p>\n<table style=\"width: 100%;\">\n<tbody>\n<tr>\n<td style=\"width: 171px; text-align: center;\" rowspan=\"2\">\n<p>\u538b\u6c5e\u4eea<\/p>\n<\/td>\n<td style=\"width: 303px; text-align: center;\" rowspan=\"2\">\n<p>\u9ea6\u514bAutoPore IV 9500<\/p>\n<\/td>\n<td style=\"width: 252px; text-align: center;\">\n<p>\u56fa\u4f53<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 252px; text-align: center;\">\n<p>\u7c89\u672b<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 171px; text-align: center;\" rowspan=\"3\">\n<p>\u692d\u504f\u4eea<\/p>\n<\/td>\n<td style=\"width: 303px; text-align: center;\" rowspan=\"3\">\n<p>\u7f8e\u56fdJ.A.Woollam\u516c\u53f8\u00a0 VB-400<\/p>\n<\/td>\n<td style=\"width: 252px; text-align: center;\">\n<p>\u8584\u819c\u539a\u5ea6<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 252px; text-align: center;\">\n<p>\u6298\u5c04\u7387<\/p>\n<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 252px; text-align: center;\">\n<p>\u6d88\u5149\u7cfb\u6570\u6d4b\u8bd5<\/p>\n<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p>\u7a46\u65af\u5821\u5c14\u8c31\u3001\u7eb3\u7c73\u538b\u75d5\u3001VSM\u3001DMA\u3001PL\u91cf\u5b50\u4ea7\u7387\u3001\u8367\u5149\u5bff\u547d\u3001NMR\u4e00\u5927\u6ce2\u8bbe\u5907\u6b63\u5728\u4e0a\u67b6\u3002\u3002\u3002\u3002\u3002<\/p>\n<p>\u4e0d\u4ec5\u5982\u6b64\uff0c\u6d4b\u8bd5\u8c37\u62e5\u6709\u4f17\u591a\u4fe1\u606f\u6765\u6e90\uff0c\u76ee\u524d\u5bf9\u4e8e\u6211\u4eec\u6682\u65f6\u672a\u80fd\u63d0\u4f9b\u7684\u6d4b\u8bd5\u8868\u5f81\u6216\u6570\u636e\u5206\u6790\u7b49\u670d\u52a1\uff0c\u90fd\u4f1a\u5411\u5ba2\u6237\u63d0\u4f9b\u4f18\u8d28\u670d\u52a1\u5546\uff0c\u6b22\u8fce\u5927\u5bb6\u54a8\u8be2\u5c0f\u8c37\uff0c\u4e5f\u6b22\u8fce\u5404\u5927\u68c0\u6d4b\u4e2d\u5fc3\u3001\u8bfe\u9898\u7ec4\u3001\u5de5\u7a0b\u5e08\u4e0e\u6211\u4eec\u5efa\u7acb\u8054\u7cfb\u3002<\/p>\n<p>\u626b\u7801\u52a0\u5165\u6750\u6599\u4eba\u5206\u6790\u6d4b\u8bd5\u7fa4\uff0c\u4e00\u6ce2\u6ce2\u7684\u8d44\u6e90\u3001\u5e72\u8d27\u548c\u57f9\u8bad\u6559\u7a0b\u6b63\u5728\u88ad\u6765\uff1a<\/p>\n<p><a href=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/03\/ceshi.png\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-71593\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/03\/ceshi.png\" alt=\"\" width=\"300\" height=\"411\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/03\/ceshi.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/03\/ceshi-219x300.png 219w\" sizes=\"(max-width: 300px) 100vw, 300px\" \/><\/a><\/p>\n<p>\u00a0\u8054\u7cfb\u65b9\u5f0f\uff1a<\/p>\n<p>QQ\uff1a3234370334 \u00a0\u6635\u79f0\uff1a\u6d4b\u8bd5\u8c37\u5b98\u65b9\u8d26\u53f7<\/p>\n<p>\u7535\u8bdd\uff1a010-57429831<\/p>\n<p>\u5fae\u4fe1\uff1aiceshigu<\/p>\n<p>\u5fae\u4fe1\u516c\u4f17\u5e73\u53f0\uff1a<a href=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/03\/\u6d4b\u8bd5\u8c37-1.jpg\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-71572\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/03\/\u6d4b\u8bd5\u8c37-1.jpg\" alt=\"\" width=\"172\" height=\"172\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/03\/\u6d4b\u8bd5\u8c37-1.jpg 172w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/03\/\u6d4b\u8bd5\u8c37-1-150x150.jpg 150w\" sizes=\"(max-width: 172px) 100vw, 172px\" \/><\/a><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u6c89\u8ff7\u79d1\u7814\u7684\u4f60\u53ef\u80fd\u9700\u8981\u4e00\u6b21\u5bf9\u5e38\u7528\u4eea\u5668\u4fe1\u606f\u3001\u5e38\u89c1\u578b\u53f7\u4ee5\u53ca\u53ef\u6d4b\u53c2\u6570\u7b80\u5355\u7c97\u66b4\u7684\u79d1\u666e\uff0c\u6765\uff0c\u6536\u4e0b\u8fd9\u4efd\u5e72\u8d27\uff01 \u968f\u540e\u5c0f\u7f16\u5c06\u901a\u8fc7\u5bf9\u6bd4\u7684\u65b9\u5f0f\u4ecb\u7ecd\u5404\u79cd\u8868\u5f81\u65b9\u5f0f\u7684\u5f02\u540c\uff0c\u4e00\u8d77\u63a2\u8ba8\u5982\u4f55\u73a9\u8f6c&#8230;<\/p>\n","protected":false},"author":51,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[4],"tags":[],"class_list":["post-71569","post","type-post","status-publish","format-standard","hentry","category-ganhuo"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/71569"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/51"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=71569"}],"version-history":[{"count":14,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/71569\/revisions"}],"predecessor-version":[{"id":71594,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/71569\/revisions\/71594"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=71569"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=71569"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=71569"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}