{"id":74900,"date":"2017-04-08T06:30:45","date_gmt":"2017-04-07T22:30:45","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=74900"},"modified":"2017-04-07T11:46:10","modified_gmt":"2017-04-07T03:46:10","slug":"%e5%8c%a1%e4%bb%a3%e5%bd%ac%e6%95%99%e6%8e%88%e7%bb%84%e6%9c%80%e6%96%b0%e8%bf%9b%e5%b1%95%ef%bc%9a%e6%97%a0%e6%9c%ba%e5%8d%a4%e5%8c%96%e9%93%85%e9%93%af%e7%ba%b3%e7%b1%b3%e7%ba%bf%e5%9f%ba%e9%95%bf","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=74900","title":{"rendered":"\u5321\u4ee3\u5f6c\u6559\u6388\u7ec4\u6700\u65b0\u8fdb\u5c55\uff1a\u65e0\u673a\u5364\u5316\u94c5\u94ef\u7eb3\u7c73\u7ebf\u57fa\u957f\u671f\u7a33\u5b9a\u7684\u9499\u949b\u77ff\u592a\u9633\u7535\u6c60"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/p>\n<p>\u8fd1\u5e74\u6765\uff0c\u4ee5\u7898\u5316\u94c5\u7532\u80fa(MAPbI<sub>3<\/sub>)\u4e3a\u4ee3\u8868\u7684\u6709\u673a\u65e0\u673a\u6742\u5316\u9499\u949b\u77ff\u6750\u6599\u56e0\u5176\u5236\u5907\u6210\u672c\u4f4e\u3001\u9ad8\u5438\u5149\u5ea6\u3001\u957f\u7535\u5b50\/\u7a7a\u7a74\u6269\u6563\u8ddd\u79bb\u7b49\u4f18\u5f02\u7684\u5149\u7535\u7279\u6027\u53d7\u5230\u5e7f\u6cdb\u5173\u6ce8\u3002\u77ed\u77ed\u51e0\u5e74\u5185\uff0c\u9499\u949b\u77ff\u592a\u9633\u7535\u6c60\u7684\u5149\u7535\u8f6c\u6362\u6548\u7387\u5c31\u5df2\u8d85\u8fc722.1%\uff0c\u5448\u73b0\u51fa\u53ef\u89c2\u7684\u7ade\u4e89\u529b\u3002\u4f46\u662f\uff0c\u7531\u4e8e\u5364\u5316\u94c5\u5e26\u9699\u5bbd\u3001\u5bfc\u7535\u6027\u5dee\u7b49\u5f31\u70b9\uff0c\u7898\u5316\u94c5\u7532\u80fa\u7b49\u6709\u673a\u65e0\u673a\u6742\u5316\u9499\u949b\u77ff\u6750\u6599\u5bf9\u6e7f\u5ea6\u3001\u70ed\u3001\u5149\u7167\u7684\u4e0d\u7a33\u5b9a\u6027\u9650\u5236\u4e86\u5176\u8fdb\u4e00\u6b65\u53d1\u5c55\u3002\u76f8\u6bd4\u4e8e\u6709\u673a\u65e0\u673a\u6742\u5316\u9499\u949b\u77ff\uff0c\u5404\u7c7b\u5168\u65e0\u673a\u5364\u5316\u94c5\u94ef\u9499\u949b\u77ff(CsPbX<sub>3<\/sub>)\u5177\u6709\u66f4\u4f18\u8d8a\u7684\u7a33\u5b9a\u6027\uff0c\u4e14\u901a\u8fc7\u8c03\u63a7\u6709\u5e8f\u7684\u5f62\u8c8c\uff0c\u53ef\u4ee5\u6709\u6548\u52a0\u5feb\u7535\u5b50\u4f20\u8f93\uff0c\u6291\u5236\u7535\u8377\u91cd\u7ec4\uff0c\u4ece\u800c\u8fdb\u4e00\u6b65\u63d0\u5347\u5176\u5149\u7535\u6027\u80fd\u3002\u56e0\u800c\u5728\u9499\u949b\u77ff\u592a\u9633\u7535\u6c60\u3001\u53d1\u5149\u5668\u4ef6\u3001\u5149\u7535\u63a2\u6d4b\u5668\u7b49\u5149\u7535\u9886\u57df\u5177\u6709\u5e7f\u9614\u7684\u5e94\u7528\u524d\u666f\u3002\u5176\u4e2d\uff0c\u5728\u5bfc\u7535\u57fa\u5e95\u4e0a\u65e0\u8868\u9762\u6d3b\u6027\u5242\u6dfb\u52a0\uff0c\u539f\u4f4d\u5408\u6210\u5168\u65e0\u673a\u5364\u5316\u94c5\u94ef\u9499\u949b\u77ff(CsPbX<sub>3<\/sub>)\u6750\u6599\u5c24\u4e3a\u91cd\u8981\u3002<\/p>\n<p><strong>\u3010\u6587\u7ae0\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u00a02017\u5e744\u6708\u53d1\u8868\u4e8e\u300a\u4e2d\u56fd\u79d1\u5b66\uff1a\u6750\u6599\u79d1\u5b66\u300b\uff08Science China Materials\uff0c\u7b80\u79f0SCMs\uff09\uff0c\u539f\u9898\u4e3a\uff1a<strong><em>Inorganic cesium lead halide CsPbX3 nanowires for long-term stable solar cells. <\/em><\/strong><\/p>\n<p><strong>\u3010\u4eae\u70b9\u3011<\/strong><\/p>\n<p>\u8fd1\u671f\uff0c<strong>\u4e2d\u5c71\u5927\u5b66\u5316\u5b66\u5b66\u9662\u5321\u4ee3\u5f6c\u6559\u6388\u8bfe\u9898\u7ec4<\/strong>\u5229\u7528\u7b80\u5355\u7684\u6eb6\u6db2\u6d78\u6ce1\u6cd5\u5728\u900f\u660e\u5bfc\u7535\u73bb\u7483\u57fa\u5e95\u4e0a\u5236\u5907\u4e86\u76f4\u5f84\u4e3a50\u2013100 nm\u7684CsPbI<sub>3<\/sub>\u7eb3\u7c73\u7ebf\uff0c\u5e76\u901a\u8fc7\u79bb\u5b50\u4ea4\u6362\u6cd5\u5728\u4e24\u5206\u949f\u5185(\u5c06CsPbI<sub>3<\/sub>\u7eb3\u7c73\u7ebf\u6d78\u6ce1\u5728CsBr\u7684\u7532\u9187\u6eb6\u6db2\u4e2d)\u6210\u529f\u5c06\u975e\u9499\u949b\u77ff\u76f8\u7684CsPbI<sub>3<\/sub>\u7f6e\u6362\u4e3a\u9499\u949b\u77ff\u76f8\u7684CsPbBr<sub>3<\/sub>\u7eb3\u7c73\u7ebf\u3002\u968f\u540e\uff0c\u4f5c\u8005\u5229\u7528\u7c89\u672bX\u5c04\u7ebf\u884d\u5c04\u3001\u7d2b\u5916\u53ef\u89c1\u5438\u6536\u5149\u8c31\u3001\u8367\u5149\u53d1\u5149\u5149\u8c31\u7b49\u8868\u5f81\u624b\u6bb5\u8be6\u7ec6\u7814\u7a76\u4e86CsPbI<sub>3<\/sub>\u4e2d\u7898\u79bb\u5b50\u4e0e\u6eb4\u79bb\u5b50\u7684\u4ea4\u6362\u8fc7\u7a0b\u3002\u7814\u7a76\u7ed3\u679c\u8868\u660e\uff0c\u5728CsPbI<sub>3<\/sub>\u5411CsPbBr<sub>3<\/sub>\u7eb3\u7c73\u7ebf\u8f6c\u6362\u8fc7\u7a0b\u4e2d\uff0c\u9664\u4e86I\u5230Br\u7684\u5364\u7d20\u79bb\u5b50\u4ea4\u6362\u4e4b\u5916\u8fd8\u4f34\u968f\u7740\u6676\u4f53\u7ed3\u6784\u7684\u53d8\u5316\u3002\u79bb\u5b50\u4ea4\u6362\u524dCsPbI<sub>3<\/sub>\u7eb3\u7c73\u7ebf\u4e3a\u975e\u9499\u949b\u77ff\u7ed3\u6784\uff0c\u5e26\u9699\u503c\u7ea6\u4e3a2.7 eV\uff0c\u5438\u5149\u8303\u56f4\u7a84\uff0c\u800cBr\u79bb\u5b50\u4ea4\u6362\u540e\u6240\u5f97\u7684CsPbBr<sub>3<\/sub>\u7eb3\u7c73\u7ebf\u4e3a\u9499\u949b\u77ff\u7ed3\u6784\uff0c\u5e26\u9699\u4e3a2.3 eV\uff0c\u6709\u6548\u6269\u5bbd\u4e86\u6750\u6599\u7684\u5438\u5149\u8303\u56f4\u3002\u5229\u7528\u4ea4\u6362\u524d\u7684CsPbI<sub>3<\/sub>\u548c\u4ea4\u6362\u540e\u7684CsPbBr<sub>3<\/sub>\u7eb3\u7c73\u7ebf\u4f5c\u4e3a\u5149\u5438\u6536\u5c42\u6240\u5236\u5907\u7684\u5e73\u9762\u7ed3\u6784\u9499\u949b\u77ff\u592a\u9633\u80fd\u7535\u6c60\uff0c\u5728\u7a7a\u6c14\u4e2d\u6697\u6001\u4e0b\u653e\u7f6e5500\u5c0f\u65f6\u540e\uff0c\u5149\u7535\u8f6c\u6362\u6548\u7387\u51e0\u4e4e\u6ca1\u6709\u8870\u51cf\uff0c\u663e\u793a\u51fa\u4e86\u53ef\u559c\u7684\u957f\u671f\u7a33\u5b9a\u6027\u3002\u8be5\u5de5\u4f5c\u63d0\u51fa\u4e86\u4e00\u79cd\u7b80\u4fbf\u6709\u6548\u7684\u65b9\u6cd5\uff0c\u5b9e\u73b0\u4e86\u5927\u9762\u79ef\u5236\u5907\u5168\u65e0\u673a\u5364\u5316\u94c5\u94ef\u9499\u949b\u77ff\u7eb3\u7c73\u7ebf\uff0c\u5177\u6709\u4f18\u5f02\u7684\u957f\u671f\u7a33\u5b9a\u6027\uff0c\u4e14\u53ef\u6269\u5c55\u5230\u5176\u4ed6\u6709\u673a\u9633\u79bb\u5b50\u3001\u65e0\u94c5\u9499\u949b\u77ff\u7b49\u6750\u6599\u7684\u4ea4\u6362\u5e94\u7528\u4e2d\uff0c\u4e3a\u9499\u949b\u77ff\u6750\u6599\u5728\u53d1\u5149\u5668\u4ef6\u3001\u5149\u7535\u63a2\u6d4b\u5668\u53ca\u5149\u50ac\u5316\u7b49\u9886\u57df\u7684\u5e94\u7528\u5960\u5b9a\u4e86\u57fa\u7840\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-74976\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/\u56fe\u72472-1.png\" alt=\"\" width=\"600\" height=\"266\" \/><\/p>\n<p style=\"text-align: center;\">\u56fe1. (a) CsPbX<sub>3<\/sub> \u7eb3\u7c73\u7ebf\u7684\u5408\u6210\u793a\u610f\u56fe\uff1bSEM\u5f62\u8c8c\u56fe (b) HPbI<sub>3<\/sub>\u819c (c) CsPbI<sub>3<\/sub>\u7eb3\u7c73\u7ebf\u8584\u819c (d) CsPbBr<sub>3<\/sub> \u7eb3\u7c73\u7ebf\u8584\u819c\uff08\u6bd4\u4f8b\u5c3a\u4e3a200 nm\uff09<\/p>\n<p>\u5728FTO\u73bb\u7483\u57fa\u5e95\u4e0a\u5229\u7528\u6eb6\u6db2\u6d78\u6e0d\u6cd5\u5408\u6210CsPbI<sub>3<\/sub>\u7eb3\u7c73\u7ebf\uff0c\u4ee5HPbI<sub>3<\/sub>\u6eb6\u6db2\u4e3a\u524d\u4f53\u65cb\u6d82\uff0c\u5e76\u6d78\u6ce1\u4e8eCsI\u7532\u9187\u6eb6\u6db2\u4e2d\uff0c\u5f97\u5230CsPbI3\u7eb3\u7c73\u7ebf\u8584\u819c\u3002\u5c55\u73b0\u4e86\u76f4\u5f84\u4e3a50-100 nm\uff0c\u5fae\u7c73\u7ea7\u957f\u5ea6\u7684\u5f62\u8c8c\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-74977\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/\u56fe\u72473-1.png\" alt=\"\" width=\"600\" height=\"477\" \/><\/p>\n<p style=\"text-align: center;\">\u56fe2. XRD \u56fe\u8c31\uff08CsPbI<sub>3 <\/sub>\u548c CsPbBr<sub>3<\/sub>\uff09<\/p>\n<p style=\"text-align: left;\">XRD\u56fe\u8c31\u4e2dCsPbI<sub>3<\/sub>\u5177\u6709\u975e\u9499\u949b\u77ff\u76f8\u7684\u7ed3\u6784\uff0c\u800cCsPbBr<sub>3<\/sub>\u5219\u5c55\u73b0\u4e86\u5178\u578b\u7684\u9499\u949b\u77ff\u7ed3\u6784\u3002<\/p>\n<p style=\"text-align: center;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-74978\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/\u56fe\u72474.png\" alt=\"\" width=\"600\" height=\"228\" \/>\u56fe3. (a) CsPbI<sub>3<\/sub>\u7eb3\u7c73\u7ebf\u8584\u819cCsBr\u7532\u9187\u6eb6\u6db2\u4e2d\u6d78\u6ce1\u4e0d\u540c\u65f6\u95f4\u7684XRD\u56fe\u8c31\uff1b(b) CsPI<sub>3<\/sub> \u548c CsPbBr<sub>3<\/sub>\u6d78\u6ce160s\u7684XRD\u56fe\u8c31\u5bf9\u6bd4<\/p>\n<p>\u968f\u6d78\u6ce1\u65f6\u95f4\u589e\u52a0\uff0cXRD\u7279\u5f81\u5cf0\u53d1\u751f\u660e\u663e\u53d8\u5316\uff0c\u8868\u793a\u65b0\u7ed3\u6784\u7684\u9010\u6e10\u751f\u6210\uff0c2 min\u65f6\uff0c\u5236\u5f97\u7eaf\u51c0\u7684\u9499\u949b\u77ff\u76f8CsPbB<sub>r3<\/sub>\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-74979\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/\u56fe\u72475.png\" alt=\"\" width=\"600\" height=\"423\" \/><\/p>\n<p style=\"text-align: center;\">\u56fe4. \u7ed3\u6784\u8f6c\u5316\u793a\u610f\u56fe<\/p>\n<p style=\"text-align: left;\">\u4ee530s\uff0c90s\uff0c2min\u4e3a\u65f6\u95f4\u8282\u70b9\uff0c\u5364\u5316\u7269\u7684\u7ed3\u6784\u5b8c\u6210\u4e86\u4ece\u975e\u9499\u949b\u77ff\u76f8\u3001\u4e24\u76f8\u5171\u5b58\u5230\u5b8c\u5168\u9499\u949b\u77ff\u7ed3\u6784\u7684\u8f6c\u5316\u8fc7\u7a0b\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-74980\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/\u56fe\u72476.png\" alt=\"\" width=\"600\" height=\"221\" \/><\/p>\n<p style=\"text-align: center;\">\u56fe5. CsPbI<sub>3<\/sub> \u7eb3\u7c73\u7ebf\u8584\u819c\u4e0d\u540c\u6d78\u6ce1\u65f6\u95f4 (a) \u5438\u6536\u5149\u8c31\uff1b(b) \u6807\u51c6\u8367\u5149\u5149\u8c31<\/p>\n<p style=\"text-align: left;\">\u6d78\u6ce1\u65f6\u95f4\u4e0d\u540c\uff0c\u6837\u54c1\u7684\u5438\u5149\u8303\u56f4\u4e0d\u540c\uff0c\u5176\u4e2d\u4e24\u76f8\u5171\u5b58\u7684\u4e2d\u95f4\u4ea7\u7269\u5438\u5149\u8303\u56f4\u6700\u5bbd\uff0c\u4e14\u901a\u8fc7\u63a7\u5236\u6d78\u6ce1\u65f6\u95f4\uff0c\u4ea7\u7269\u7684\u5e26\u9699\u53ef\u8c03\u8c10\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-74981\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/\u56fe\u72477.png\" alt=\"\" width=\"600\" height=\"235\" \/><\/p>\n<p style=\"text-align: center;\">\u56fe6. (a) \u9499\u949b\u77ff\u592a\u9633\u80fd\u7535\u6c60\u7684J-V\u8868\u5f81\uff1b(b) \u57fa\u4e8eCsPbBr<sub>3<\/sub>\u7eb3\u7c73\u7ebf\u592a\u9633\u80fd\u7535\u6c60\u7684\u622a\u9762\u548c\u5e73\u9762SEM\u5f62\u8c8c\u56fe<\/p>\n<p style=\"text-align: center;\">\u88681. \u9499\u949b\u77ff\u592a\u9633\u80fd\u7535\u6c60\u7684\u5668\u4ef6\u53c2\u6570<\/p>\n<p style=\"text-align: center;\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone  wp-image-74921\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/\u56fe\u72475-2-300x44.jpg\" alt=\"\" width=\"436\" height=\"64\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/\u56fe\u72475-2-300x44.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/\u56fe\u72475-2-768x113.jpg 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/\u56fe\u72475-2-1024x151.jpg 1024w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/\u56fe\u72475-2.jpg 1483w\" sizes=\"(max-width: 436px) 100vw, 436px\" \/><\/p>\n<p style=\"text-align: left;\">\u5404\u9879\u8868\u5f81\u6307\u6807\u8868\u660e\uff0c\u79bb\u5b50\u4ea4\u6362\u5b8c\u6210\u540e\uff0c\u7535\u6c60\u6027\u80fd\u63d0\u9ad8\u4e86\u8fd110\u500d\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-74982\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/\u56fe\u72478.png\" alt=\"\" width=\"600\" height=\"450\" \/><\/p>\n<p style=\"text-align: center;\">\u56fe7. \u8001\u5316\u65f6\u95f4<\/p>\n<p style=\"text-align: left;\">\u5728\u7a7a\u6c14\u4e2d\u6697\u6001\u4e0b\u653e\u7f6e5500\u5c0f\u65f6\u540e\uff0c\u5149\u7535\u8f6c\u6362\u6548\u7387\u51e0\u4e4e\u6ca1\u6709\u8870\u51cf\uff0c\u8868\u73b0\u4e86\u4f18\u5f02\u7684\u7a33\u5b9a\u6027\uff0c\u8fdb\u4e00\u6b65\u62d3\u5c55\u4e86\u65e0\u673a\u9499\u949b\u77ff\u592a\u9633\u80fd\u7535\u6c60\u7684\u5e94\u7528\u8303\u56f4\u3002<\/p>\n<p><strong>\u3010\u5c0f\u7ed3\u3011<\/strong><\/p>\n<p>\u5728\u5982\u4f55\u539f\u4f4d\u5408\u6210\u5168\u65e0\u673a\u5364\u5316\u94c5\u94ef\u9499\u949b\u77ff(CsPbX<sub>3<\/sub>)\u6750\u6599\u7684\u95ee\u9898\u4e0a\uff0c\u5321\u4ee3\u5f6c\u6559\u6388\u8bfe\u9898\u7ec4\u62a5\u9053\u4e86\u7b80\u4fbf\u7684\u6eb6\u6db2\u6d78\u6e0d\u6cd5\u548c\u5364\u7d20\u4ea4\u6362\u6280\u672f\uff0c\u5236\u5f97\u4e86CsPbI<sub>3 <\/sub>\u548c CsPbBr<sub>3 <\/sub>\u7eb3\u7c73\u7ebf\u3002\u4f7f\u7528\u5404\u9879\u8868\u5f81\u9a8c\u8bc1\u4e86\u975e\u9499\u949b\u77ff\u7ed3\u6784\u5230\u9499\u949b\u77ff\u7ed3\u6784\u7684\u6210\u529f\u8f6c\u5316\uff0c\u5149\u7535\u8f6c\u5316\u6548\u7387\u8fbe\u5230\u4e861.21%\uff0c\u4e14\u5c55\u73b0\u4e86\u4f18\u5f02\u7684\u7a33\u5b9a\u6027\u3002\u540c\u65f6\uff0c\u8be5\u5de5\u4f5c\u63d0\u51fa\u4e86\u4e00\u79cd\u65e0\u673a\u9499\u949b\u77ff\u7eb3\u7c73\u7ebf\u6db2\u76f8\u539f\u4f4d\u5408\u6210\u6cd5\uff0c\u6709\u76ca\u4e8e\u534a\u900f\u660e\u9499\u949b\u77ff\u592a\u9633\u80fd\u7535\u6c60\u3001\u5149\u7535\u63a2\u6d4b\u5668\u53ca\u5176\u4ed6\u5149\u7535\u5668\u4ef6\u7684\u8fdb\u4e00\u6b65\u53d1\u5c55\u3002<\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5\uff1a<\/strong><a href=\"http:\/\/engine.scichina.com\/publisher\/scp\/journal\/SCMs\/doi\/10.1007\/s40843-016-5131-9\">Inorganic cesium lead halide CsPbX3 nanowires for long-term stable solar cells (Sci. China. Mater., 2016, DOI: 10.1007\/s40843-017-9014-9)<\/a><\/p>\n<p><strong>\u3010\u671f\u520a\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u300a\u4e2d\u56fd\u79d1\u5b66\uff1a\u6750\u6599\u79d1\u5b66\u300b\uff08Science China Materials\uff0c\u7b80\u79f0SCMs\uff09\u521b\u520a\u4e8e2014\u5e74\u5e95\uff0c\u7531\u4e2d\u56fd\u79d1\u5b66\u9662\u548c\u56fd\u5bb6\u81ea\u7136\u79d1\u5b66\u57fa\u91d1\u59d4\u5458\u4f1a\u5171\u540c\u4e3b\u529e\uff0c\u662f\u300a\u4e2d\u56fd\u79d1\u5b66\u300b\u7cfb\u5217\u671f\u520a\u4e4b\u4e00\uff0c\u73b0\u5df2\u88abSCI\u6536\u5f55\u3002SCMs\u4ee5\u5feb\u901f\u53d1\u8868\u6750\u6599\u79d1\u5b66\u6700\u65b0\u91cd\u8981\u7814\u7a76\u6210\u679c\u4e3a\u529e\u520a\u5b97\u65e8\uff0c\u4e3a\u6750\u6599\u79d1\u5b66\u548c\u5316\u5b66\u3001\u7269\u7406\u3001\u751f\u547d\u79d1\u5b66\u7b49\u76f8\u5173\u5b66\u79d1\u7684\u79d1\u7814\u4eba\u5458\u63d0\u4f9b\u4e86\u4e00\u4e2a\u53ca\u65f6\u4ea4\u6d41\u79d1\u7814\u6210\u679c\u4e0e\u601d\u60f3\u7684\u65b0\u5e73\u53f0\u3002SCMs\u6db5\u76d6\u4e86\u6750\u6599\u79d1\u5b66\u7814\u7a76\u7684\u5404\u4e2a\u9886\u57df\uff0c\u5c24\u5176\u4fa7\u91cd\u4e8e\u5f53\u524d\u7684\u70ed\u70b9\u7814\u7a76\u65b9\u5411\uff0c\u5982\u80fd\u6e90\u5b58\u50a8\u6750\u6599\u3001\u50ac\u5316\u6750\u6599\u3001\u751f\u7269\u6750\u6599\u3001\u7eb3\u7c73\u7ed3\u6784\u548c\u529f\u80fd\u6027\u6750\u6599\u7b49\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u8fd1\u5e74\u6765\uff0c\u4ee5\u7898\u5316\u94c5\u7532\u80fa(MAPbI3)\u4e3a\u4ee3\u8868\u7684\u6709\u673a\u65e0\u673a\u6742\u5316\u9499\u949b\u77ff\u6750\u6599\u56e0\u5176\u5236\u5907\u6210\u672c\u4f4e\u3001\u9ad8\u5438\u5149\u5ea6\u3001\u957f\u7535\u5b50\/\u7a7a\u7a74\u6269\u6563\u8ddd\u79bb\u7b49\u4f18\u5f02\u7684\u5149\u7535\u7279\u6027\u53d7\u5230\u5e7f\u6cdb\u5173\u6ce8\u3002\u77ed\u77ed\u51e0\u5e74&#8230;<\/p>\n","protected":false},"author":3554,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[78,33],"class_list":["post-74900","post","type-post","status-publish","format-standard","hentry","category-jiedu","tag-photovoltaic","tag-nano"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/74900"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/3554"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=74900"}],"version-history":[{"count":2,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/74900\/revisions"}],"predecessor-version":[{"id":74922,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/74900\/revisions\/74922"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=74900"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=74900"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=74900"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}