{"id":78030,"date":"2017-04-29T14:00:54","date_gmt":"2017-04-29T06:00:54","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=78030"},"modified":"2017-05-04T18:11:48","modified_gmt":"2017-05-04T10:11:48","slug":"corros-sci-%ef%bc%9abe%e5%92%8cca%e5%af%b9%e6%8f%90%e9%ab%98%e9%95%81%e5%90%88%e9%87%91mg-9al-1zn%e7%9a%84%e9%ab%98%e6%b8%a9%e6%8a%97%e6%b0%a7%e5%8c%96%e6%80%a7%e7%9a%84%e7%bb%84%e5%90%88%e5%bd%b1","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=78030","title":{"rendered":"Corros. Sci.\uff1aBe\u548cCa\u5bf9\u63d0\u9ad8\u9541\u5408\u91d1Mg-9Al-1Zn\u7684\u9ad8\u6e29\u6297\u6c27\u5316\u6027\u7684\u7ec4\u5408\u5f71\u54cd"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/p>\n<p>\u9541\u5408\u91d1(Mg)\u4f5c\u4e3a\u91cd\u8981\u7684\u8f7b\u8d28\u9ad8\u5f3a\u6750\u6599\uff0c\u88ab\u5e7f\u6cdb\u5e94\u7528\u4e8e\u6c7d\u8f66\u548c\u822a\u7a7a\u9886\u57df\u3002\u7136\u800c\uff0c\u5176\u5de8\u5927\u5e94\u7528\u53d7\u5236\u4e8e\u5176\u8f83\u62b5\u7684\u6297\u9ad8\u6e29\u6c27\u5316\u6027\uff08\u9ad8\u4e8e400\u2103\uff09\u3002\u5f53\u6e29\u5ea6\u8f83\u9ad8\u65f6\uff0c\u5176\u8868\u9762\u53d1\u751f\u4e25\u91cd\u9000\u5316\u751a\u81f3\u5f15\u8d77\u706b\u707e\u3002\u636e\u62a5\u9053\uff0c\u5f53\u9541\u5408\u91d1\u4e2d\u542b\u6709\u5fae\u91cf\u7684\u94cd\uff08Be\uff09\u5143\u7d20\u65f6\uff0c\u53ef\u5728\u9541\u5408\u91d1\u8868\u9762\u5f62\u6210BeO\u5c42\uff0c\u4ece\u800c\u663e\u8457\u63d0\u9ad8\u5176\u6297\u9ad8\u6e29\u6c27\u5316\u6027\u3002\u7136\u800c\uff0cBe\u4e0d\u4ec5\u6602\u8d35\u800c\u4e14\u6709\u6bd2, \u53e6\u4e00\u79cd\u529e\u6cd5\u662f\u63ba\u9499\uff08Ca\uff09\uff0c\u4e5f\u53ef\u901a\u8fc7\u5f62\u6210\u5bccCaO\u5c42\u6765\u63d0\u9ad8\u6297\u9ad8\u6e29\u6c27\u5316\u6027\u3002\u7136\u800c\uff0c\u76ee\u524d\u5bf9\u4e8e\u8fd9\u4e24\u79cd\u5143\u7d20\u7684\u4f5c\u7528\u6548\u679c\u3001\u5dee\u5f02\u4ee5\u53ca\u7ec4\u5408\u5f71\u54cd\u9541\u5408\u91d1\u6297\u6c27\u5316\u6027\u884c\u4e3a\u90fd\u6709\u5f85\u7814\u7a76\u3002\u4e3a\u6b64\uff0c\u672c\u6587\u901a\u8fc7\u540c\u65f6\u63ba\u5165Be\u548cCa\uff0c\u6765\u7814\u7a76\u5176\u7ec4\u5408\u6297\u9ad8\u6e29\u6c27\u5316\u6027\u80fd\uff0c\u4ece\u800c\u51cf\u5c11Be\u5728\u6297\u6c27\u5316\u9541\u5408\u91d1\u4e2d\u7684\u4f7f\u7528\u3002<\/p>\n<p>\n <strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c<strong>\u7531\u6fb3\u5927\u5229\u4e9a\u6606\u58eb\u5170\u5927\u5b66\u6750\u6599\u79d1\u5b66\u4e0e\u5de5\u7a0b\u7684\u5f20\u660e\u661f\u6559\u6388(\u901a\u8baf\u4f5c\u8005)\u5728Corrosion Science<\/strong>\u4e0a\u5728\u7ebf\u53d1\u8868\u4e86\u4e00\u7bc7\u540d\u4e3a \u201c<strong> Combined influence of Be and Ca on improving the high-temperature oxidation resistance of the magnesium alloy Mg-9Al-1Zn<\/strong> \u201d \u7684\u6587\u7ae0\u3002\u6587\u4e2d\uff0c\u7814\u7a76\u4eba\u5458\u901a\u8fc7\u5728Mg-9Al-1Zn\uff08AZ91\uff09\u5408\u91d1\u4e2d\u63ba\u5165\u4e00\u5b9a\u91cf\u7684Be \u548cCa\u5143\u7d20\uff0c\u53d1\u73b0\u542b\u670920 ppm (wt)\u7684Be and \u548c0.5 wt.% \u7684Ca\u7684AZ91\u9541\u5408\u91d1\u7684\u6297\u6c27\u5316\u6027\u6bd4\u542b\u670960 ppm (wt) \u7684Be\u7684AZ91\u66f4\u9ad8\uff0c\u5e76\u7814\u7a76\u5f97\u5230\u5176\u4f5c\u7528\u673a\u7406\uff1a\uff08a\uff09\u5728\u5408\u91d1\u8868\u9762\u5f62\u6210\u4e86\u4e00\u79cdBe\u589e\u5f3a\u578b\u7684CaO-MgO\u590d\u5408\u5c42\uff1b\uff08b\uff09\u901a\u8fc7\u5982\u4e0b\u4e24\u79cd\u65b9\u6cd5\u6765\u6291\u5236\u9541\u5408\u91d1\u5728\u6676\u754c\u5904\u7684\u84b8\u53d1: (i)\u6d88\u9664Mg-Al\u5171\u6676\u5fae\u7ec4\u5206\uff1b(ii) Ca\u5408\u91d1\u5316\uff0c\u4f7f\u03b2-Mg17Al12\u7684\u70ed\u7a33\u5b9a\u6027\u589e\u52a0\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p><strong>\u56fe1. \u71c3\u70b9\u6e29\u5ea6\u6d4b\u91cf\u5b9e\u9a8c\u88c5\u7f6e\u793a\u610f\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-78031\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/tu1-2.jpg\" alt=\"\" width=\"600\" height=\"287\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/tu1-2.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/tu1-2-300x144.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n \u5c06\u6837\u54c1\u7f6e\u4e8e\u5177\u6709\u7ebf\u6027\u5347\u6e29\u7684\u9876\u5f00\u5f0f\u7535\u963b\u7089\u4e2d\u7684\u5769\u57da\u4e2d\u52a0\u70ed\uff0c\u901a\u8fc7\u6837\u54c1\u6e29\u5ea6\u7684\u6025\u5267\u589e\u52a0\u6765\u786e\u5b9a\u7740\u706b\u6e29\u5ea6\u3002<\/p>\n<p><strong>\u56fe2. AZ91\u548cAZ91Be60\u9541\u5408\u91d1\u7684\u7ec4\u7ec7\u548c\u6210\u5206\u5206\u6790<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-78032\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/2-49.jpg\" alt=\"\" width=\"600\" height=\"466\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/2-49.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/2-49-300x233.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u56fe\uff08a\uff09\u548c\u56fe\uff08b\uff09\u5206\u522b\u4e3aAZ91\u548cAZ91Be60\u9541\u5408\u91d1\u7684\u573a\u53d1\u5c04\u626b\u63cf\u7535\u5b50\u663e\u5fae\u56fe\u50cf\uff08FESEM\uff09\u548c\u76f8\u5bf9\u5e94\u7684\u5143\u7d20\u9762\u626b\u80fd\u8c31\u56fe\uff08EDS\uff09\u3002\u4ece\u4e2d\u53ef\u770b\u51fa\uff0c\u4e24\u79cd\u6750\u6599\u90fd\u4ee5\u03b1-Mg\u4f5c\u4e3a\u57fa\u4f53\uff0c\u4ee5\u03b1-Mg +\u03b2-Mg17Al12\u91d1\u5c5e\u95f4\u5316\u5408\u7269\u5f62\u6210\u5c42\u72b6\u5171\u6676\u7ec4\u7ec7\u3002\u52a0\u516560 ppm (wt) Be\u5e76\u6ca1\u6709\u663e\u8457\u6539\u53d8AZ91\u9541\u5408\u91d1\u7684\u539f\u6709\u94f8\u6001\u7ec4\u7ec7\u5f62\u6001\u3002<\/p>\n<p><strong>\u56fe3. AZX910\u548cAZX911\u9541\u5408\u91d1\u7684\u7ec4\u7ec7\u548c\u6210\u5206\u5206\u6790<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-78033\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/3-43.jpg\" alt=\"\" width=\"600\" height=\"466\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/3-43.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/3-43-300x233.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u56fe\uff08a\uff09\u548c\u56fe\uff08b\uff09\u5206\u522b\u4e3aAZX910\u548cAZX911\u9541\u5408\u91d1\u7684\u573a\u53d1\u5c04\u626b\u63cf\u7535\u5b50\u663e\u5fae\u56fe\u50cf\uff08FESEM\uff09\u548c\u76f8\u5bf9\u5e94\u7684\u5143\u7d20\u9762\u626b\u80fd\u8c31\u56fe\uff08EDS\uff09\u3002\u4ece\u4e2d\u53ef\u4ee5\u770b\u5230\uff0c\u5728\u8fd9\u4e24\u79cd\u5408\u91d1\u4e2d\uff0c\u5c42\u72b6\u5206\u5e03\u7684Mg-Al\u5171\u6676\u7ec4\u7ec7\u660e\u663e\u51cf\u5c11\u3002\u5f53Ca\u542b\u91cf\u8fbe\u52301.0%\u8d28\u91cf\u6bd4\u91cd\u65f6\uff0c\u5728AZX911\u5408\u91d1\u4e2d\u7684\u03b2-Mg17Al12 \u91d1\u5c5e\u95f4\u5316\u5408\u7269\u6240\u5360\u4f53\u79ef\u5206\u6570\u663e\u8457\u964d\u4f4e\u3002\u53e6\u5916\uff0c\u5b58\u5728\u9879\u94fe\u72b6\u7684Al2Ca \u91d1\u5c5e\u95f4\u5316\u5408\u7269\u548c\u5c42\u72b6\u7684Mg-Al2Ca\u5171\u6676\u7ec4\u7ec7\u6cbf\u679d\u6676\u8fb9\u754c\u5206\u5e03\u3002<\/p>\n<p><strong>\u56fe4. AZX910Be60\u548cAZX911Be60\u9541\u5408\u91d1\u7684\u7ec4\u7ec7\u548c\u6210\u5206\u5206\u6790<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-78034\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/4-41.jpg\" alt=\"\" width=\"600\" height=\"471\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/4-41.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/4-41-300x236.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u00a0\u56fe\uff08a\uff09\u548c\u56fe\uff08b\uff09\u5206\u522b\u4e3aAZX910Be60 \u548cAZX911Be60 \u9541\u5408\u91d1\u7684\u573a\u53d1\u5c04\u626b\u63cf\u7535\u5b50\u663e\u5fae\u56fe\u50cf\uff08FESEM\uff09\u548c\u76f8\u5bf9\u5e94\u7684\u5143\u7d20\u9762\u626b\u80fd\u8c31\u56fe\uff08EDS\uff09\u3002\u4ece\u4e2d\u53ef\u4ee5\u770b\u5230\uff0c\u542b60 ppm (wt) Be\u7684\u8fd9\u4e24\u79cd\u5408\u91d1\u90fd\u6ca1\u6709\u663e\u8457\u6539\u53d8\u539f\u6709\u94f8\u6001\u7ec4\u7ec7\u7684\u5f62\u6001\u3002\u53e6\u5916\uff0c\u5728EDS\u7684\u6d4b\u91cf\u7cbe\u5ea6\u8303\u56f4\u5185\uff0c\u7531\u4e8eBe\u542b\u91cf\u8f83\u5c11\uff0c\u5728\u94f8\u6001\u5408\u91d1\u4e2d\u6ca1\u68c0\u6d4b\u5230Be\u3002<\/p>\n<p><strong>\u56fe5. \u70ed\u91cd\u5206\u6790<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-78035\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/5-31.jpg\" alt=\"\" width=\"550\" height=\"800\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/5-31.jpg 550w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/5-31-206x300.jpg 206w\" sizes=\"(max-width: 550px) 100vw, 550px\" \/><br \/>\n \uff08a\uff09\u548c\u56fe\uff08b\uff09\u5206\u522b\u4e3a\u542b\u6709\u5404\u79cdCa\u548cBe\u5143\u7d20\u542b\u91cf\u7684\u7cfb\u5217\u94f8\u6001AZ91 \u9541\u5408\u91d1\u5206\u522b\u5728400\u2103\u548c450\u2103\u4e0b\u7684\u70ed\u91cd\u6570\u636e\u3002\u4ece\u4e2d\u53ef\u4ee5\u770b\u5230\uff0c\u968f\u7740\u65f6\u95f4\u7684\u5ef6\u957f\uff0c\u5408\u91d1\u7684\u603b\u8d28\u91cf\u662f\u4e0d\u65ad\u589e\u52a0\u7684\uff0c\u8868\u660e\u53d1\u751f\u4e86\u6c27\u5316\u3002\u5e76\u4e14\u52a0\u5165\u6709Ca\u548cBe\u5143\u7d20\u7684\u5408\u91d1\u5728\u8fd9\u4e24\u79cd\u5b9e\u9a8c\u6e29\u5ea6\u4e0b\u90fd\u53ef\u4ee5\u4e0d\u540c\u7a0b\u5ea6\u7684\u964d\u4f4e\u589e\u91cd\u901f\u7387\uff0c\u8bf4\u660e\u53ef\u964d\u4f4e\u6c27\u5316\u901f\u7387\u964d\u4f4e\uff0c\u65e2\u8d77\u5230\u4e00\u5b9a\u7684\u6297\u6c27\u5316\u4f5c\u7528\u3002\u542b20ppm\uff08wt\uff09Be\u548c0.5wt\uff05Ca\u7684\u534f\u540c\u6548\u5e94\u4e0e\u542b60ppm\uff08wt\uff09Be\u7684\u6548\u679c\u76f8\u4f3c\u3002<\/p>\n<p><strong>\u56fe6. \u5b8f\u89c2\u5f62\u8c8c<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-78036\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/6-23.jpg\" alt=\"\" width=\"550\" height=\"551\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/6-23.jpg 550w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/6-23-150x150.jpg 150w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/6-23-300x300.jpg 300w\" sizes=\"(max-width: 550px) 100vw, 550px\" \/><\/p>\n<p>\u5404\u79cd\u6210\u5206\u542b\u91cf\u7684\u9541\u5408\u91d1\u5728\u6e29\u5ea6400\u2103\u7684\u7089\u5185\u6c27\u5316144h\u540e\u7684\u5b8f\u89c2\u5f62\u8c8c\u3002\u4ece\u4e2d\u53ef\u4ee5\u770b\u5230\uff0c\u5404\u7cfb\u5217\u7684AZ91, AZX910\u548cAZX911 \u9541\u5408\u91d1\u90fd\u88ab\u4e25\u91cd\u6c27\u5316\u3002\u5176\u4e2d\u8868\u9762\u4e0a\u7684\u9ed1\u8272\u7247\u533a\u4ee3\u8868\u7740\u6709\u8f83\u539a\u53ca\u975e\u7c98\u9644\u6c27\u5316\u7269\u5c42\u7684\u5f62\u6210\u3002\u5728AZX910Be10 \u548cAZ91Be60\u9541\u5408\u91d1\u8868\u9762\u4e0a\u6709\u6c27\u5316\u7269\u7ed3\u8282\uff0c\u610f\u5473\u7740\u5b58\u5728\u7740\u6c27\u5316\u819c\u5f00\u88c2\u3002 AZX910Be20, AZX911Be10, AZX911Be20, AZX910Be60 \u548c AZX911Be60 \u8fd9\u4e94\u79cd\u542bBe\u7684\u9541\u5408\u91d1\u90fd\u5f97\u5230\u4e86\u8f83\u597d\u7684\u4fdd\u62a4\uff0c\u5373\u6709\u7740\u8f83\u9ad8\u7684\u6297\u6c27\u5316\u6027\u80fd\uff0c\u8bf4\u660e\u52a0\u5165Be\u53ef\u4ee5\u663e\u8457\u63d0\u9ad8AZ91\u9541\u5408\u91d1\u7684\u6297\u6c27\u5316\u6027\u80fd\u3002<\/p>\n<p><strong>\u56fe7. \u71c3\u70b9\u6e29\u5ea6<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-78037\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/7-16.jpg\" alt=\"\" width=\"550\" height=\"490\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/7-16.jpg 550w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/7-16-300x267.jpg 300w\" sizes=\"(max-width: 550px) 100vw, 550px\" \/><\/p>\n<p>\u8be5\u56fe\u4e3a\u5404\u9541\u5408\u91d1\u8bd5\u6837\u5728\u52a0\u70ed\u901f\u7387\u4e3a5\u2103\/min\u6761\u4ef6\u4e0b\u6d4b\u91cf\u5f97\u5230\u7684\u71c3\u70b9\u6e29\u5ea6\u3002\u4ece\u4e2d\u53ef\u4ee5\u770b\u5230\uff0c\u52a0\u5165Ca \u548c Be\u5143\u7d20\u90fd\u6709\u52a9\u4e8e\u63d0\u9ad8\u9541\u5408\u91d1\u7684\u71c3\u70b9\u6e29\u5ea6\u3002\u5f53AZ91\u9541\u5408\u91d1\u4e2d\u52a0\u51650.5wt.\uff05\u7684Ca\u548c20ppm\uff08wt\uff09\u7684Be\u7684\u63d0\u5347\u71c3\u70b9\u6e29\u5ea6\u7684\u7ec4\u5408\u6548\u679c\u6bd4\u5355\u4e00\u52a0\u51651.0wt.\uff05\u7684Ca\u621660ppm\uff08wt\uff09\u7684Be\u7684\u6548\u679c\u90fd\u8981\u9ad8\u3002<\/p>\n<p><strong>\u56fe8. \u5404\u9541\u5408\u91d1\u8bd5\u6837\u6c27\u5316\u7269\u5c42\u7684\u6a2a\u622a\u9762\u5f62\u8c8c<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-78038\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/8-14.jpg\" alt=\"\" width=\"550\" height=\"413\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/8-14.jpg 550w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/8-14-300x225.jpg 300w\" sizes=\"(max-width: 550px) 100vw, 550px\" \/><\/p>\n<p>\u56fe\uff08a\uff09,\uff08b\uff09,\uff08c\uff09,\uff08d\uff09\u5206\u522b\u4e3aAZ91\uff0c AZ91Be60\uff0cAZX911\uff0cAZX911Be60\u9541\u5408\u91d1\u5728\u7a7a\u6c14\u4e2d400\u2103\u6761\u4ef6\u4e0b\u7089\u5185\u6c27\u5316144h\u540e\u7684\u6c27\u5316\u7269\u5c42\u7684\u6a2a\u622a\u9762\u5f62\u8c8c\u3002\u4ece\u4e2d\u53ef\u4ee5\u770b\u5230\uff0cCa\u548cBe\u5143\u7d20\u7684\u52a0\u5165\u6709\u52a9\u4e8e\u9541\u5408\u91d1\u8868\u9762\u5f62\u6210\u81f4\u5bc6\u548c\u7d27\u51d1\u7684\u6c27\u5316\u7269\u5c42\u3002<\/p>\n<p><strong>\u56fe9. \u5404\u9541\u5408\u91d1\u5dee\u70ed\u5206\u6790\uff08DTA\uff09<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-78039\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/9-11.jpg\" alt=\"\" width=\"550\" height=\"427\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/9-11.jpg 550w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/9-11-300x233.jpg 300w\" sizes=\"(max-width: 550px) 100vw, 550px\" \/><\/p>\n<p>\u8be5\u56fe\u4e3aAZ91, AZ91Be60, AZX911\u548cAZX911Be60 \u56db\u79cd\u9541\u5408\u91d1\u5728\u52a0\u70ed\u901f\u7387\u4e3a10 K\/min\u65f6\u7684\u5dee\u70ed\u5206\u6790\uff08DTA\uff09\u66f2\u7ebf. \u4ece\u4e2d\u53ef\u4ee5\u770b\u5230\uff0c\u5f53AZ91\u9541\u5408\u91d1\u4e2d\u52a0\u51651.0 wt.% \u7684Ca\u540e\uff0c\u5176\u7194\u70b9\u63d0\u9ad830\u2103\u3002\u76f8\u6bd4\u4e4b\u4e0b\uff0cBe\u7684\u52a0\u5165\u5bf9AZ91Be60, AZX911Be60 \u4e24\u79cd\u542bBe\u5408\u91d1\u7684DTA\u66f2\u7ebf\u7684\u5f71\u54cd\u90fd\u5f88\u5c0f\u3002<\/p>\n<p><strong>\u56fe10. AZX911Be60\u5408\u91d1\u6c27\u5316\u7269\u5c42\u6f14\u53d8\u793a\u610f\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-78040\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/10-8.jpg\" alt=\"\" width=\"600\" height=\"338\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/10-8.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/10-8-300x169.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n \uff08a\uff09\u5728\u521d\u59cb\u6c27\u5316\u9636\u6bb5\uff0c\u5728\u91d1\u5c5e\u8868\u9762\u5f62\u6210\u8584\u7684MgO\u5c42\u3002<br \/>\n \uff08b\uff09\u7531\u4e8eMg2 +\u7684\u5411\u5916\u6269\u6563\uff0cBe\u52a0\u5f3a\u81f4\u5bc6\u578b\u7684MgO\u5c42\u5728\u521d\u59cb\u5f62\u6210\u7684\u6c27\u5316\u5c42\u4e0a\u7ee7\u7eed\u751f\u957f\u3002 \u540c\u65f6\uff0cCa2 +\u5728\u91d1\u5c5e\/\u6c27\u5316\u7269\u754c\u9762\u7684\u79ef\u7d2f\u5bfc\u81f4\u5f62\u6210\u5bccCa\u533a\u3002<br \/>\n \uff08c\uff09CaO \/ MgO\u590d\u5408\u5c42\u5f62\u6210\u5728\u81f4\u5bc6\u7684MgO\u5c42\u4e4b\u4e0b\uff0c\u63d0\u4f9b\u989d\u5916\u7684\u6297\u6c27\u5316\u6027\u4fdd\u62a4\u3002<\/p>\n<p><strong>\u88681. \u5404\u9541\u5408\u91d1\u8bd5\u6837\u901a\u8fc7\u7535\u611f\u8026\u5408\u7b49\u79bb\u5b50\u4f53-\u539f\u5b50\u53d1\u5c04\u5149\u8c31\u4eea\uff08ICP-AES\uff09\u6d4b\u51fa\u7684\u5408\u91d1\u6210\u5206\u5206\u6790\uff08wt. % \u6216 wt. ppm\uff09\u548c\u71c3\u70b9\u6e29\u5ea6\u3002<\/strong><\/p>\n<p><a href=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/\u88681-2.bmp\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-78042\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/\u88681-2.bmp\" alt=\"\" width=\"620\" height=\"226\" \/><\/a><\/p>\n<p><strong>\u88682. \u56fe8\u6240\u6307\u533a\u57df\u901a\u8fc7EDS\u6d4b\u51fa\u7684\u5143\u7d20\u6210\u5206(wt. %)<\/strong><\/p>\n<p><a href=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/\u56fe\u72473-2.bmp\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-78044\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/04\/\u56fe\u72473-2.bmp\" alt=\"\" width=\"681\" height=\"255\" \/><\/a><br \/>\n <strong>\u3010\u5c0f\u7ed3\u3011<\/strong><\/p>\n<p>\u672c\u5b9e\u9a8c\u901a\u8fc7\u5bf9AZ91\u9541\u5408\u91d1\u5206\u522b\u52a0\u5165\u4e0d\u540c\u542b\u91cf\u7684\u7684Be\uff0cCa\u5143\u7d20\uff0c\u5e76\u5bf9\u5176\u8fdb\u884c\u76f8\u5e94\u7684\u6027\u80fd\u6d4b\u8bd5\u548c\u8868\u5f81\uff0c\u7ed3\u5408\u5f62\u8c8c\u548c\u65ad\u9762\u5206\u6790\uff0c\u5f97\u51fa\u5982\u4e0b\u7ed3\u8bba\uff1a\uff081\uff09\u4e0eBe\u548cCa\u7684\u5355\u4e00\u5408\u91d1\u5316\u76f8\u6bd4\uff0cBe\u548cCa\u7684\u7ec4\u5408\u5408\u91d1\u5316\u53ef\u4ee5\u66f4\u6709\u6548\u5730\u63d0\u9ad8AZ91\u7684\u6297\u6c27\u5316\u6027\u548c\u71c3\u70b9\u6e29\u5ea6\u3002\u5e76\u53d1\u73b0\u542b60ppm \uff08wt\uff09Be\u548c1.0wt.\uff05Ca\uff0c\u53ef\u4f7f\u9541\u5408\u91d1\u83b7\u5f97\u6700\u9ad8\u7684\u6297\u6c27\u5316\u6027\u3002\u53e6\u5916\uff0c\u52a0\u51650.5wt\uff05\u7684Ca\u80fd\u591f\u663e\u7740\u964d\u4f4e\u6602\u8d35\u4e14\u6709\u6bd2\u7684Be\u542b\u91cf\uff1b \uff082\uff09\u63d0\u51fa\u4e86\u4e00\u79cd\u5173\u4e8eBe\u5408\u91d1\u63d0\u9ad8\u6297\u6c27\u5316\u6027\u7684\u5047\u8bbe\uff1aMgO\u5c42\u53ef\u4ee5\u901a\u8fc7\u5f62\u6210Be-MgO\u56fa\u6eb6\u4f53\u6216\u6cbf\u7740MgO\u6676\u754c\u901a\u8fc7\u201cREE\u201d\u6765\u589e\u5f3a\u3002\u8fdb\u800c\u5f62\u6210\u66f4\u7d27\u51d1\u7684MgO\u5c42\uff0c\u63d0\u9ad8\u5176\u8fdb\u4e00\u6b65\u6297\u6c27\u5316\u7684\u80fd\u529b\uff1b \uff083\uff09Ca\u5408\u91d1\u5316\u80fd\u591f\u5728AZ91\u5408\u91d1\u7684\u8868\u9762\u5f62\u6210CaO \/ MgO\u590d\u5408\u6c27\u5316\u7269\u5c42\uff0c\u66f4\u52a0\u7d27\u51d1\u548c\u66f4\u575a\u56fa\uff0c\u83b7\u5f97\u66f4\u9ad8\u7684\u6297\u6c27\u5316\u80fd\u529b\uff1b \uff084\uff09Be\u548cCa \u7684\u7ec4\u5408\u5408\u91d1\u5316\u4f7fAZ91\u5408\u91d1\u83b7\u5f97\u7ec4\u5408\u6297\u6c27\u5316\u6027\u3002\u5176\u673a\u7406\u4e3a\uff1a\u6291\u5236Mg\u84b8\u53d1\u548c\u5f62\u6210\u7531\u5916\u90e8\u589e\u5f3a\u7684MgO\u5c42\u548c\u5185\u90e8CaO \/ MgO\u590d\u5408\u5c42\u7ec4\u6210\u7684\u81f4\u5bc6\u7684\u53cc\u76f8\u6c27\u5316\u7269\u5c42\u3002\u53cc\u76f8\u5c42\u53ef\u4f5c\u4e3aMg\u7684\u5411\u5916\u84b8\u53d1\u548c\u6c27\u5411\u5185\u6e17\u900f\u7684\u58c1\u5792\uff0c\u4ece\u800c\u5b9e\u73b0\u9ad8\u6297\u6c27\u5316\u6027\u3002<\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5\uff1a<\/strong> <a href=\"http:\/\/www.sciencedirect.com\/science\/article\/pii\/S0010938X1730094X\" target=\"_blank\" rel=\"noopener noreferrer\">Combined influence of Be and Ca on improving the high-temperature oxidation resistance of the magnesium alloy Mg-9Al-1Zn<\/a>\u00a0\uff08Corros. Sci.\uff1a2017\uff0cDOI.org\/10.1016\/j.corsci.2017.03.023\uff09<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u7f16\u8f91\u90e8<strong>\u91d1\u5c5e\u6750\u6599\u5b66\u672f\u7ec4\u5f6d\u9ec4\u6d9b\u4f9b\u7a3f\uff0c\u6750\u6599\u725b\u7f16\u8f91\u6574\u7406<\/strong>\u3002\u6b22\u8fce\u52a0\u5165\u6750\u6599\u4eba\u7f16\u8f91\u90e8\u91d1\u5c5e\u6750\u6599\u5b66\u672f\u4ea4\u6d41\u7fa4\uff08458281221\uff09\uff01<\/p>\n<p>\u6750\u6599\u725b\u7f51\u4e13\u6ce8\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u53ca\u884c\u4e1a\u8fdb\u5c55\uff0c\u8fd9\u91cc\u6c47\u96c6\u4e86\u5404\u5927\u9ad8\u6821\u7855\u535a\u751f\u3001\u4e00\u7ebf\u79d1\u7814\u4eba\u5458\u4ee5\u53ca\u884c\u4e1a\u4ece\u4e1a\u8005\uff0c\u5982\u679c\u60a8\u5bf9\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u8fdb\u5c55\uff0c\u89e3\u8bfb\u9ad8\u6c34\u5e73\u6587\u7ae0\u6216\u662f\u8bc4\u8ff0\u884c\u4e1a\u6709\u5174\u8da3\uff0c<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\" target=\"_blank\" rel=\"noopener noreferrer\">\u70b9\u6211\u52a0\u5165\u6750\u6599\u4eba\u7f16\u8f91\u90e8<\/a>\u3002<\/p>\n<p><strong><span style=\"color: #ff0000;\">\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1axiaofire-18\uff0c\u5434\u73ab\uff0c\u6211\u4eec\u4f1a\u62c9\u5404\u4f4d\u8001\u5e08\u52a0\u5165\u4e13\u5bb6\u7fa4\u3002<\/span><\/strong><\/p>\n<p><strong>\u6750\u6599\u6d4b\u8bd5\uff0c\u6570\u636e\u5206\u6790\uff0c<a href=\"http:\/\/www.ceshigu.com\/\" target=\"_blank\" rel=\"noopener noreferrer\">\u4e0a\u6d4b\u8bd5\u8c37<\/a>\uff01<\/strong><\/p>\n<p>\u6750\u6599\u4eba\u7f51\u5c0a\u91cd\u6240\u6709\u8fdb\u884c\u77e5\u8bc6\u4f20\u64ad\u7684\u5a92\u4f53\uff0c\u8f6c\u8f7d\u8bf7\u8054\u7cfbtougao@cailiaoren.com\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u9541\u5408\u91d1(Mg)\u4f5c\u4e3a\u91cd\u8981\u7684\u8f7b\u8d28\u9ad8\u5f3a\u6750\u6599\uff0c\u88ab\u5e7f\u6cdb\u5e94\u7528\u4e8e\u6c7d\u8f66\u548c\u822a\u7a7a\u9886\u57df\u3002\u7136\u800c\uff0c\u5176\u5de8\u5927\u5e94\u7528\u53d7\u5236\u4e8e\u5176\u8f83\u62b5\u7684\u6297\u9ad8\u6e29\u6c27\u5316\u6027\uff08\u9ad8\u4e8e400\u2103\uff09\u3002\u5f53\u6e29\u5ea6\u8f83\u9ad8\u65f6\uff0c\u5176\u8868\u9762\u53d1\u751f&#8230;<\/p>\n","protected":false},"author":2756,"featured_media":78045,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[90,981],"class_list":["post-78030","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-jiedu","tag-craft","tag-test"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/78030"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/2756"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=78030"}],"version-history":[{"count":13,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/78030\/revisions"}],"predecessor-version":[{"id":79153,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/78030\/revisions\/79153"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/78045"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=78030"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=78030"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=78030"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}