{"id":90096,"date":"2017-07-08T14:00:05","date_gmt":"2017-07-08T06:00:05","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=90096"},"modified":"2017-07-07T13:26:15","modified_gmt":"2017-07-07T05:26:15","slug":"nano-lett-%ef%bc%9a%e7%9f%b3%e5%a2%a8%e7%83%af%e8%96%84%e8%86%9c%e7%9a%84%e5%a4%96%e5%bb%b6%e7%94%9f%e9%95%bf%e5%8f%8a%e5%b8%a6%e7%bb%93%e6%9e%84","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=90096","title":{"rendered":"Nano lett.\uff1a\u77f3\u58a8\u70ef\u8584\u819c\u7684\u5916\u5ef6\u751f\u957f\u53ca\u5e26\u7ed3\u6784"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/p>\n<p>\u77f3\u58a8\u70ef\u7684\u53d1\u73b0\u6fc0\u53d1\u4e86\u5bf9\u57fa\u672c\u4e8c\u7ef4\uff082D\uff09\u6750\u6599\u7684\u7814\u7a76\u7684\u5de8\u5927\u5174\u8da3\uff0c\u5177\u6709\u4e0e\u5176\u5927\u91cf\u5bf9\u5e94\u7269\u4e0d\u540c\u7684\u5916\u6765\u7269\u7406\u548c\u5316\u5b66\u6027\u8d28\u3002\u4f7f\u7528\u5206\u5b50\u675f\u5916\u5ef6\uff0c\u89c2\u5bdf\u5230\u7684\u975e\u51e1\u7684\u7535\u5b50\u7ed3\u6784\u5c55\u793a\u4e86\u5176\u5728\u672a\u6765\u7eb3\u7c73\u5668\u4ef6\u548c\u5149\u7535\u5668\u4ef6\u5e94\u7528\u4e2d\u7684\u524d\u666f\u3002\u4f53\u79ef\u5355\u6676Te\u662f\u7a84\u5e26\u9699\u534a\u5bfc\u4f53\uff080.33eV\uff09\u7684\u7406\u8bba\u7814\u7a76\u63d0\u51fa\u4e86\u5355\u5c42Te\uff0c\u03b1-Te\uff0c\u03b2-Te\u548c\u03b3-Te\u7684\u4e09\u79cd\u7ed3\u6784\u7c7b\u578b\uff0c\u5176\u4e2d\u03b1-Te\u548c\u03b2-Te\u5206\u522b\u4e3a\u5e26\u9699\u4e3a0.75\u548c1.47eV\u7684\u534a\u5bfc\u4f53\u3002\u56e0\u6b64\uff0c\u63a7\u5236\u539a\u5ea6\u53ef\u4ee5\u5b9e\u73b0\u4ece\u4e2d\u7ea2\u5916\uff080.3eV\uff09\u5230\u8fd1\u7ea2\u5916\uff081.5eV\uff09\u7684\u91cd\u8981\u5149\u8c31\u8303\u56f4\u7684Te\u819c\u4e0b\u964d\u5230\u5355\u4e2a\u539f\u5b50\u5c42\u3002\u53e6\u4e00\u65b9\u9762\uff0c\u7531\u4e8eTe\u539f\u5b50\u6570\u76f8\u5bf9\u8f83\u9ad8\uff0cTe\u539f\u5b50\u8868\u73b0\u51fa\u5f3a\u70c8\u7684\u81ea\u65cb\u8f68\u9053\u8026\u5408\u3002\u5728\u5916\u90e8\u5e94\u53d8\u4e0b\uff0c\u901a\u8fc7\u7406\u8bba\u7814\u7a76\u9884\u6d4b\u4e86Te\u5355\u6676\u7684\u62d3\u6251\u76f8\u53d8\u3002\u53e6\u5916\uff0c\u901a\u8fc7\u5149\u7535\u5b50\u80fd\u8c31\u9274\u5b9a\u7684\u5927\u91cf\u65b0\u578b\u91cf\u5b50\u6750\u6599\uff0c\u4f8b\u5982\u62d3\u6251\u7edd\u7f18\u5b50Bi\/Sb<sub>2<\/sub>Te<sub>3<\/sub>\u548cZrTe<sub>5<\/sub>\u548c\u62d3\u6251\u534a\u91d1\u5c5eW\/MoTe<sub>2<\/sub>\u90fd\u5177\u6709Te\u539f\u5b50\u5c42\u4f5c\u4e3a\u6784\u4ef6\uff0c\u6fc0\u53d1\u4e86\u5bf9\u5355\u5c42Te\u8584\u819c\u7684\u5e7f\u6cdb\u7814\u7a76\u5174\u8da3\u3002\u7136\u800c\uff0c\u9664\u4e86\u901a\u8fc7\u5404\u79cd\u65b9\u6cd5\u5b9e\u73b0\u7684\u4e0d\u540c\u7c7b\u578b\u7684Te\u7eb3\u7c73\u7ed3\u6784\u5916\uff0c\u62a5\u9053\u4e86Te\u819c\u7684\u5916\u5ef6\u751f\u957f\uff0c\u539f\u5b50\u5c3a\u5ea6\u4e0a\u7684\u8868\u5f81\u4ecd\u7136\u4e0d\u5b58\u5728\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c<strong>\u4e2d\u79d1\u9662\u7269\u7406\u6240\u738b\u709c\u534e\u548c\u90ed\u5efa\u4e1c\uff08\u5171\u540c\u901a\u8baf\u4f5c\u8005\uff09\u8bfe\u9898\u7ec4\u5728Nano lett.<\/strong>\u4e0a\u53d1\u8868\u4e86\u9898\u4e3a\u201c<strong>Epitaxial Growth and Band Structure of Te Film on Graphene<\/strong>\u201d \u7684\u6587\u7ae0\u3002\u8be5\u7814\u7a76\u56e2\u961f\u901a\u8fc7MBE\u62a5\u544a6H-SiC\uff080001\uff09\u886c\u5e95\u4e0a\u77f3\u58a8\u70ef\u8868\u9762\u4e0aTe\u819c\u7684\u8303\u5fb7\u534e\u529b\uff08vdW\uff09\u5916\u5ef6\u3002\u5728\u5355\u5c42\u548c\u51e0\u5c42\u8584\u819c\u4e2d\u83b7\u5f97\u4e86Te\u7684\u4e8c\u7ef4\u5f62\u5f0f\u3002\u901a\u8fc7\u626b\u63cf\u96a7\u9053\u663e\u5fae\u955c\uff08STM\uff09\u7814\u7a76\uff0c\u63ed\u793a\u4e86Te\u819c\u7531\u5e73\u884c\u6392\u5217\u7684\u87ba\u65cbTe\u94fe\u7ec4\u6210\uff0c\u5e73\u5766\u5730\u8eba\u5728\u77f3\u58a8\u70ef\u8868\u9762\u4e0a\uff0c\u9732\u51fa\u6563\u88c5Te\u6676\u4f53\u7684\uff08101\u03050\uff09\u7684\uff081\u00d71\uff09\u9762\u3002\u901a\u8fc7\u626b\u63cf\u96a7\u9053\u663e\u5fae\u955c\uff08STS\uff09\u6d4b\u91cf\uff0cTe\u819c\u7684\u5e26\u9699\u968f\u7740\u539a\u5ea6\u4ece0.33eV\uff08\u4f53\u79ef\uff09\u964d\u4f4e\u81f30.92eV\uff08\u5355\u5c42\uff09\u800c\u5355\u8c03\u589e\u52a0\uff0c\u8986\u76d6\u4ece\u4e2d\u7ea2\u5916\u5230\u8fd1\u7ea2\u5916\u7684\u5149\u8c31\u8303\u56f4\u3002\u6b64\u5916\uff0c\u7a7a\u95f4\u5206\u8fa8\u7684STS\u5149\u8c31\u663e\u793a\u5411\u4e0a\u7684\u5e26\u5f2f\u66f2\uff0c\u5bfc\u81f4\u5728\u5355\u5c42Te\u548c\u77f3\u58a8\u70ef\u7684\u8fb9\u754c\u5904\u7684\u7a7a\u7a74\u79ef\u805a\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p><strong>\u56fe<\/strong><strong>1 <\/strong><strong>\u77f3\u58a8\u70ef\u4e0a<\/strong><strong>Te<\/strong><strong>\u8584\u819c\u7684\u5730\u5f62\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-90101\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/07\/nl-2017-01029g_0001.jpeg\" alt=\"\" width=\"700\" height=\"674\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/07\/nl-2017-01029g_0001.jpeg 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/07\/nl-2017-01029g_0001-300x289.jpeg 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>\uff08a\uff09\u5927\u9762\u79ef\u7684STM\u56fe\u50cf\uff083.125V\/50pA\uff09\u7684\u751f\u957f\u7684Te\u819c\u5206\u5e03\u5728\u57fa\u677f\uff08SiC\uff09\u6b65\u9aa4\uff08\u84dd\u8272\u7bad\u5934\u6240\u793a\uff09\u4e0a\uff1b<\/p>\n<p>\uff08b\uff09\u5355\u5c42Te\u819c\u7684\u9ad8\u5206\u8fa8\u7387STM\u56fe\u50cf\uff081.5V\/30pA\uff09\uff1b<\/p>\n<p>\uff08c\uff09\uff086\u00d76\uff09\u91cd\u6784\u77f3\u58a8\u70ef\uff08\u56fe\u50cf\u7684\u4e0a\u90e8\uff09\u4e0e\u5355\u5c42Te\u819c\uff08\u56fe\u50cf\u7684\u4e0b\u90e8\uff09\u4e4b\u95f4\u7684\u6b65\u957f\u7684STM\u56fe\u50cf\uff1b<\/p>\n<p>\uff08d\u548ce\uff09\u5206\u522b\u5982\u56fec\u6240\u793a\u7684\u77f3\u58a8\u70ef\u548c\u5355\u5c42Te\u7684\u5feb\u901f\u5085\u7acb\u53f6\u53d8\u6362\u56fe\u6848\u3002<\/p>\n<p><strong>\u56fe<\/strong><strong>2<\/strong><strong> D34<\/strong><strong>\uff08<\/strong><strong>152<\/strong><strong>\uff03\uff09\u4e09\u89d2\u7a7a\u95f4\u7ec4\u7684<\/strong><strong>Te<\/strong><strong>\u5355\u6676\u6676\u683c\u7ed3\u6784<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-90103\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/07\/nl-2017-01029g_0002.jpeg\" alt=\"\" width=\"700\" height=\"263\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/07\/nl-2017-01029g_0002.jpeg 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/07\/nl-2017-01029g_0002-300x113.jpeg 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>\uff08a\uff093D\u7ed3\u6784\u793a\u610f\u56fe\uff1b<\/p>\n<p>\uff08b\u548cc\uff09\u5206\u522b\u4e3aa0-b0\u548cb0-c0\u5e73\u9762\uff1b<\/p>\n<p>\uff08d\uff09\u77f3\u58a8\u70ef\/SiC\uff080001\uff09\u4e0a\u65e0\u9650\u53cc\u5c42Te\u819c\u76843D\u56fe\u3002<\/p>\n<p><strong>\u56fe<\/strong><strong>3 <\/strong><strong>\u5177\u6709\u4e0d\u540c\u539a\u5ea6\u7684<\/strong><strong>Te<\/strong><strong>\u819c\u7684\u5e26\u9699\u6f14\u53d8<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-90104\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/07\/nl-2017-01029g_0003.jpeg\" alt=\"\" width=\"700\" height=\"540\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/07\/nl-2017-01029g_0003.jpeg 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/07\/nl-2017-01029g_0003-300x231.jpeg 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>\uff08a\uff09\u5728\u4e0d\u540c\u5c42\u7684\u77f3\u58a8\u70ef\/ SiC\u66b4\u9732\u68af\u7530\u4e0a\u7684Te\u5c9b\u7684\u5dee\u5206STM\u56fe\u50cf\uff1b<\/p>\n<p>\uff08b\uff09\u77f3\u58a8\u70ef\u5e95\u7269\u548c\u5355\u5c42Te\u7684dI\/dV\u5149\u8c31\uff08\u301c800mV\/100pA\uff09\uff1b<\/p>\n<p>\uff08c\uff09\u5728L2\uff0cL3\u548cL4\u4e0a\u62cd\u6444\u7684dI\/dV\u5149\u8c31\uff0c\u53ef\u4ee5\u786e\u5b9a\u5e26\u9699\uff1b<\/p>\n<p>\uff08d\uff09Te\u819c\u7684\u5e26\u9699\u4f5c\u4e3a\u539a\u5ea6\u7684\u51fd\u6570\u3002<\/p>\n<p><strong>\u56fe<\/strong><strong>4 <\/strong><strong>\u6cbf\u7740\u56fe<\/strong><strong>3a<\/strong><strong>\u4e2d\u7684\u865a\u7ebf\u6a59\u7ebf\u62cd\u6444\u7684\u5dee\u5206\u7535\u5bfc\uff08<\/strong><strong>dI\/dV<\/strong><strong>\u5149\u8c31\uff09<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-90105\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/07\/nl-2017-01029g_0004.jpeg\" alt=\"\" width=\"700\" height=\"350\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/07\/nl-2017-01029g_0004.jpeg 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/07\/nl-2017-01029g_0004-300x150.jpeg 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>\uff08a\uff09\u4ee5\u5bf9\u6570\u523b\u5ea6\uff08-1.5V\/100pA\uff0c\u8c03\u5236\u4e3a10mV\uff09\u76842D\u5f69\u8272\u6620\u5c04\u7ed8\u5236dI\/dV\u5149\u8c31\uff08\u4ee51nm\u7684\u95f4\u9694\u62cd\u6444\u768450\u6761\u66f2\u7ebf\uff09\uff1b<\/p>\n<p>\uff08b\uff09\u5728\u5177\u6709\u76f8\u540c\u989c\u8272\u7684\u9762\u677fa\u4e2d\u6807\u8bb0\u7684\u4f4d\u7f6e\u5904\u83b7\u5f97\u4ee3\u8868\u6027\u7684dI\/dV\u5149\u8c31\u3002<\/p>\n<p><strong>\u3010\u5c0f\u7ed3\u3011<\/strong><\/p>\n<p>\u8be5\u7814\u7a76\u56e2\u961f\u901a\u8fc7vdW\u5916\u5ef6\u5728\u77f3\u58a8\u70ef\/6H-SiC\uff080001\uff09\u886c\u5e95\u4e0a\u751f\u957f\u5355\u5c42\u548c\u51e0\u5c42Te\u819c\u3002\u5177\u6709\u4e0d\u540c\u539a\u5ea6\u7684Te\u8584\u819c\u6cbf[101\u03050]\u65b9\u5411\u5f62\u6210\u4e8e\u4f53\u79efTe\u6676\u4f53\u7684\u7ed3\u6784\u4e2d\uff0c\u5176\u4e2d\u87ba\u65cb\u94fe\u5e73\u5766\u5730\u4f4d\u4e8e\u6bcf\u5c42\u4e2d\u5e76\u4e14\u5f7c\u6b64\u5e73\u884c\u3002Te\u7684\u5e26\u9699\u968f\u7740\u539a\u5ea6\u7684\u589e\u52a0\u800c\u5355\u8c03\u589e\u52a0\uff0c\u5bf9\u4e8e\u5355\u5c42Te\u8fbe\u52300.92eV\u3002\u5355\u5c42Te\u548c\u77f3\u58a8\u70ef\u7684\u8fb9\u754c\u5904\u89c2\u5bdf\u5230\u5411\u4e0a\u7684\u5e26\u5f2f\u66f2\uff0c\u8868\u73b0\u51fa\u5c40\u90e8\u5b54\u79ef\u805a\u3002<\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5<\/strong>\uff1a<a href=\"http:\/\/pubs.acs.org\/doi\/10.1021\/acs.nanolett.7b01029\" target=\"_blank\" rel=\"noopener noreferrer\">Epitaxial Growth and Band Structure of Te Film on Graphene<\/a>\u00a0 \uff08Nano Lett., 2017, DOI: 10.1021\/acs.nanolett.7b01029\uff09<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u7f16\u8f91\u90e8<strong>\u7eb3\u7c73\u6750\u6599\u5b66\u672f\u7ec4\u575a\u6bc5\u4f9b\u7a3f\uff0c\u6750\u6599\u725b\u7f16\u8f91\u6574\u7406<\/strong>\u3002\u6b22\u8fce\u52a0\u5165\u6750\u6599\u4eba\u7f16\u8f91\u90e8\u7eb3\u7c73\u6750\u6599\u5b66\u672f\u4ea4\u6d41\u7fa4\uff08228686798\uff09\uff01<\/p>\n<p>\u6750\u6599\u725b\u7f51\u4e13\u6ce8\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u53ca\u884c\u4e1a\u8fdb\u5c55\uff0c\u8fd9\u91cc\u6c47\u96c6\u4e86\u5404\u5927\u9ad8\u6821\u7855\u535a\u751f\u3001\u4e00\u7ebf\u79d1\u7814\u4eba\u5458\u4ee5\u53ca\u884c\u4e1a\u4ece\u4e1a\u8005\uff0c\u5982\u679c\u60a8\u5bf9\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u8fdb\u5c55\uff0c\u89e3\u8bfb\u9ad8\u6c34\u5e73\u6587\u7ae0\u6216\u662f\u8bc4\u8ff0\u884c\u4e1a\u6709\u5174\u8da3\uff0c<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\" target=\"_blank\" rel=\"noopener noreferrer\">\u70b9\u6211\u52a0\u5165\u6750\u6599\u4eba\u7f16\u8f91\u90e8<\/a>\u3002<\/p>\n<p><strong>\u6750\u6599\u6d4b\u8bd5\uff0c\u6570\u636e\u5206\u6790<\/strong>\uff0c<a href=\"http:\/\/www.ceshigu.com\/\" target=\"_blank\" rel=\"noopener noreferrer\">\u4e0a\u6d4b\u8bd5\u8c37<\/a>\uff01<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u77f3\u58a8\u70ef\u7684\u53d1\u73b0\u6fc0\u53d1\u4e86\u5bf9\u57fa\u672c\u4e8c\u7ef4\uff082D\uff09\u6750\u6599\u7684\u7814\u7a76\u7684\u5de8\u5927\u5174\u8da3\uff0c\u5177\u6709\u4e0e\u5176\u5927\u91cf\u5bf9\u5e94\u7269\u4e0d\u540c\u7684\u5916\u6765\u7269\u7406\u548c\u5316\u5b66\u6027\u8d28\u3002\u4f7f\u7528\u5206\u5b50\u675f\u5916\u5ef6\uff0c\u89c2\u5bdf\u5230\u7684\u975e\u51e1\u7684\u7535\u5b50\u7ed3\u6784\u5c55\u793a\u4e86\u5176\u5728&#8230;<\/p>\n","protected":false},"author":3440,"featured_media":90109,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[46],"class_list":["post-90096","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-jiedu","tag-graphene"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/90096"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/3440"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=90096"}],"version-history":[{"count":5,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/90096\/revisions"}],"predecessor-version":[{"id":90385,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/90096\/revisions\/90385"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/90109"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=90096"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=90096"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=90096"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}