{"id":92592,"date":"2017-07-21T09:30:08","date_gmt":"2017-07-21T01:30:08","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=92592"},"modified":"2017-07-22T08:59:37","modified_gmt":"2017-07-22T00:59:37","slug":"science-%e9%94%82%e7%a6%bb%e5%ad%90%e7%94%b5%e6%b1%a0%e7%a1%85%e8%b4%9f%e6%9e%81%e9%87%8d%e5%a4%a7%e8%bf%9b%e5%b1%95%ef%bc%81","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=92592","title":{"rendered":"Science: \u9502\u79bb\u5b50\u7535\u6c60\u7845\u8d1f\u6781\u91cd\u5927\u8fdb\u5c55\uff01"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/p>\n<p>\u968f\u7740\u5148\u8fdb\u6750\u6599\u548c\u5168\u7535\u6c14\u5316\u7535\u52a8\u8f66\u5e94\u7528\u53d1\u5c55\u5bf9\u7535\u6c60\u9700\u6c42\u7684\u63d0\u5347\uff0c\u9502\u79bb\u5b50\u7535\u6c60\u7684\u80fd\u91cf\u5bc6\u5ea6\u4e5f\u5728\u4e0d\u65ad\u63d0\u9ad8\uff1b\u7845\u6750\u6599\u7531\u4e8e\u5176\u4f18\u5f02\u7684\u6bd4\u5bb9\u91cf\u800c\u6210\u4e3a\u4e00\u79cd\u7406\u60f3\u7684\u8d1f\u6781\u6750\u6599\u3002\u5728\u5145\u653e\u7535\u5faa\u73af\u8fc7\u7a0b\u4e2d\uff0c\u7845\u8d1f\u6781\u5b58\u5728\u660e\u663e\u7684\u4f53\u79ef\u53d8\u5316\u5bfc\u81f4\u7535\u6781\u6750\u6599\u7834\u788e\u5e76\u5f62\u6210\u4e0d\u7a33\u5b9a\u7684\u7535\u6781-\u7535\u89e3\u8d28\u754c\u9762\uff0c\u56e0\u800c\u7535\u6781\u7684\u5faa\u73af\u5bff\u547d\u53d7\u5230\u9650\u5236\u3002\u6700\u8fd1\uff0c\u7814\u7a76\u53d1\u73b0\u7535\u6781\u6750\u6599\u4e2d\u7c98\u7ed3\u5242\u7684\u4f7f\u7528\u6709\u52a9\u4e8e\u5927\u5e45\u5ea6\u63d0\u9ad8\u7535\u6781\u7684\u5faa\u73af\u5bff\u547d\uff0c\u4f46\u662f\u4f20\u7edf\u7684PVDF\u7c98\u7ed3\u5242\u4e0e\u7845\u6216\u94dc\u96c6\u6d41\u4f53\u4ec5\u4f9d\u9760\u5fae\u5f31\u7684\u8303\u5fb7\u534e\u529b\u7ed3\u5408\u800c\u4e0d\u9002\u7528\u4e8e\u7845\u8d1f\u6781\u6750\u6599\u3002<\/p>\n<p> <strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u5317\u4eac\u65f6\u95f42017\u5e747\u670821\u65e5\uff0c\u97e9\u56fd\u79d1\u5b66\u6280\u672f\u9662(KAIST)\u7684Ali Coskun\u548c Jang Wook Choi(\u5171\u540c\u901a\u8baf)\u7b49\u4eba\u4ee5\u201c<strong>Highly elastic binders integrating polyrotaxanes for silicon microparticle anodes in lithium ion batteries<\/strong>\u201d\u4e3a\u9898\u5728<strong>Science<\/strong>\u4e0a\u53d1\u8868\u6587\u7ae0\u62a5\u9053\u4e86\u4e00\u79cd\u9ad8\u5f39\u6027\u7684\u7c98\u7ed3\u5242\uff0c\u901a\u8fc7\u5f62\u6210\u916f\u952e\u4f7f\u4f20\u7edf\u7c98\u7ed3\u5242PAA\u4e0e\u591a\u805a\u8f6e\u70f7\u73af\u7ec4\u5206\u4ea4\u8054\u7ed3\u5408\u5f97\u5230\u5177\u6709\u7279\u6b8a\u7ed3\u6784\u7684\u53cc\u7ec4\u5206PR-PAA\u7c98\u7ed3\u5242\uff0c\u5f88\u5927\u7a0b\u5ea6\u4e0a\u63d0\u9ad8\u4e86\u7845\u8d1f\u6781\u5728\u5145\u653e\u7535\u8fc7\u7a0b\u4e2d\u7684\u7a33\u5b9a\u6027\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u56fe\u4e00 SiMP\u8d1f\u6781PR-PAA\u7c98\u7ed3\u5242\u7684\u5e94\u529b\u91ca\u653e\u673a\u7406<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-92609\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/07\/F1.large_-5.jpg\" alt=\"\" width=\"600\" height=\"835\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/07\/F1.large_-5.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/07\/F1.large_-5-216x300.jpg 216w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n a) \u51cf\u5c0f\u63d0\u8d77\u7269\u4f53\u7528\u529b\u7684\u6ed1\u8f6e\u673a\u7406\uff1b<\/p>\n<p>b) PR-PAA\u7c98\u7ed3\u5242\u7528\u4e8e\u7f13\u89e3\u56e0\u7845\u9897\u7c92\u5145\u653e\u7535\u8fc7\u7a0b\u4e2d\u4f53\u79ef\u53d8\u5316\u800c\u4ea7\u751f\u7684\u5e94\u529b\u793a\u610f\u56fe\uff1b<\/p>\n<p>c) \u5145\u653e\u7535\u8fc7\u7a0b\u4e2dPAA-SiMP\u7535\u6781\u7834\u788e\u548c\u4ea7\u751fSEI\u819c\u7684\u793a\u610f\u56fe\u3002<\/p>\n<p>\u56fe\u4e8c PR-PAA\u7c98\u7ed3\u5242\u7684\u673a\u68b0\u6027\u80fd<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-92610\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/07\/F2.large_-4.jpg\" alt=\"\" width=\"531\" height=\"1280\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/07\/F2.large_-4.jpg 531w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/07\/F2.large_-4-124x300.jpg 124w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/07\/F2.large_-4-425x1024.jpg 425w\" sizes=\"(max-width: 531px) 100vw, 531px\" \/><\/p>\n<p>a) \u4e09\u79cd\u5178\u578b\u6a21\u578b\u7684\u5e94\u529b-\u5e94\u53d8\u884c\u4e3a\uff1b<\/p>\n<p>b) PR-PAA\u548cPAA\u8584\u819c\u5e94\u529b-\u5e94\u53d8\u66f2\u7ebf\u7684\u5bf9\u6bd4\u548cPR-PAA\u7c98\u7ed3\u5242\u4e09\u4e2a\u5e94\u53d8\u70b9\u5904\u7684\u7f51\u7edc\u7ed3\u6784\u793a\u610f\u56fe\uff1b<\/p>\n<p>c) \u5728\u4e0d\u540c\u7684\u5e94\u53d8\u6781\u9650\u4e0b\uff0cPR-PAA 10\u6b21\u62c9\u4f38-\u56de\u590d\u5faa\u73af\u7684\u5e94\u529b-\u5e94\u53d8\u66f2\u7ebf\u3002<\/p>\n<p>\u56fe\u4e09 \u4f7f\u7528PR-PAA\u548cPAA\u7c98\u7ed3\u5242\u7684SiMP\u7535\u6781\u7535\u5316\u5b66\u6027\u80fd<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-92611\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/07\/F3.large_-5.jpg\" alt=\"\" width=\"600\" height=\"726\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/07\/F3.large_-5.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/07\/F3.large_-5-248x300.jpg 248w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>a) \u4e24\u79cd\u7c98\u7ed3\u5242\u7535\u6781\u7684\u9996\u6b21\u5145\u653e\u7535\u6027\u80fd\u6d4b\u8bd5\uff1b<\/p>\n<p>b) \u4e24\u79cd\u7c98\u7ed3\u5242\u7535\u6781\u7684\u653e\u7535\u5bb9\u91cf\u4fdd\u6301\u7387\u6d4b\u8bd5\uff1b<\/p>\n<p>c) \u57280.2C\u548c0.4C\u4e0b\u6d4b\u8bd5PR-PAA-SiMP\u7535\u6781\u7684\u653e\u7535\u5bb9\u91cf\u4fdd\u6301\u7387\u548c\u5e93\u4f26\u6548\u7387\uff1b<\/p>\n<p>d) \u57280.03C\u4e0b\uff0cSiMP-LiNi<sub>0.8<\/sub>Co<sub>0.15<\/sub>Al<sub>0.05<\/sub>O<sub>2<\/sub>\u5168\u7535\u6c60\u7684\u9996\u6b21\u5145\u653e\u7535\u6d4b\u8bd5\uff1b<\/p>\n<p>e) \u57280.2C\u4e0b\uff0cSiMP-LiNi<sub>0.8<\/sub>Co<sub>0.15<\/sub>Al<sub>0.05<\/sub>O<sub>2<\/sub>\u5168\u7535\u6c60\u7684\u5faa\u73af\u6027\u80fd\u548c\u5e93\u4f26\u6548\u7387\u3002<\/p>\n<p>\u56fe\u56db SiMP\u8d1f\u6781\u5faa\u73af\u524d\u540e\u7684\u975e\u539f\u4f4dSEM\u8868\u5f81<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-92612\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/07\/F4.large_-2.jpg\" alt=\"\" width=\"600\" height=\"639\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/07\/F4.large_-2.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/07\/F4.large_-2-282x300.jpg 282w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>a,b) PR-PAA-SiMP\u548cPAA-SiMP\u7535\u6781\u5faa\u73af\u524d\u7684\u622a\u9762SEM\u56fe\u50cf\uff1b<\/p>\n<p>c,d) PR-PAA-SiMP\u548cPAA-SiMP\u7535\u6781\u5faa\u73af10\u5708\u540e\u7684\u622a\u9762SEM\u56fe\u50cf\uff1b<\/p>\n<p>e,f) PR-PAA-SiMP\u548cPAA-SiMP\u7535\u6781\u5faa\u73af10\u5708\u540e\u7684\u4fef\u89c6SEM\u56fe\u50cf\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1a<a href=\"http:\/\/science.sciencemag.org\/content\/357\/6348\/279\" target=\"_blank\" rel=\"noopener noreferrer\">Highly elastic binders integrating polyrotaxanes for silicon microparticle anodes in lithium ion batteries<\/a>\u00a0(Science, 2017, DOI: 10.1126\/science.aal4373)<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u65b0\u80fd\u6e90\u7ec4Jane915126\u4f9b\u7a3f\uff0c\u6750\u6599\u725b\u6574\u7406\u7f16\u8f91\u3002\u53c2\u4e0e\u65b0\u80fd\u6e90\u8bdd\u9898\u8ba8\u8bba\u8bf7\u52a0\u5165\u201c\u6750\u6599\u4eba\u65b0\u80fd\u6e90\u6750\u6599\u4ea4\u6d41\u7fa4 422065952\u201d\u3002<\/p>\n<p>\u6750\u6599\u725b\u7f51\u4e13\u6ce8\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u53ca\u884c\u4e1a\u8fdb\u5c55\uff0c\u8fd9\u91cc\u6c47\u96c6\u4e86\u5404\u5927\u9ad8\u6821\u7855\u535a\u751f\u3001\u4e00\u7ebf\u79d1\u7814\u4eba\u5458\u4ee5\u53ca\u884c\u4e1a\u4ece\u4e1a\u8005\uff0c\u5982\u679c\u60a8\u5bf9\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u8fdb\u5c55\uff0c\u89e3\u8bfb\u9ad8\u6c34\u5e73\u6587\u7ae0\u6216\u662f\u8bc4\u8ff0\u884c\u4e1a\u6709\u5174\u8da3\uff0c<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\" target=\"_blank\" rel=\"noopener noreferrer\">\u70b9\u6211\u52a0\u5165\u7f16\u8f91\u90e8\u5927\u5bb6\u5ead<\/a>\u3002<\/p>\n<p><strong>\u6750\u6599\u6d4b\u8bd5\uff0c\u6570\u636e\u5206\u6790\uff0c<\/strong><a href=\"http:\/\/www.ceshigu.com\/\" target=\"_blank\" rel=\"noopener noreferrer\"><strong>\u4e0a\u6d4b\u8bd5\u8c37<\/strong><\/a><strong>\uff01<\/strong><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u968f\u7740\u5148\u8fdb\u6750\u6599\u548c\u5168\u7535\u6c14\u5316\u7535\u52a8\u8f66\u5e94\u7528\u53d1\u5c55\u5bf9\u7535\u6c60\u9700\u6c42\u7684\u63d0\u5347\uff0c\u9502\u79bb\u5b50\u7535\u6c60\u7684\u80fd\u91cf\u5bc6\u5ea6\u4e5f\u5728\u4e0d\u65ad\u63d0\u9ad8\uff1b\u7845\u6750\u6599\u7531\u4e8e\u5176\u4f18\u5f02\u7684\u6bd4\u5bb9\u91cf\u800c\u6210\u4e3a\u4e00\u79cd\u7406\u60f3\u7684\u8d1f\u6781\u6750\u6599\u3002\u5728\u5145\u653e\u7535\u5faa\u73af&#8230;<\/p>\n","protected":false},"author":369,"featured_media":92618,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215,2],"tags":[129],"class_list":["post-92592","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-jiedu","category-keji","tag-battery"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/92592"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/369"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=92592"}],"version-history":[{"count":10,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/92592\/revisions"}],"predecessor-version":[{"id":92734,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/92592\/revisions\/92734"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/92618"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=92592"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=92592"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=92592"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}