{"id":95773,"date":"2017-08-13T06:30:25","date_gmt":"2017-08-12T22:30:25","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=95773"},"modified":"2017-08-10T23:52:55","modified_gmt":"2017-08-10T15:52:55","slug":"j-am-ceram-soc-%ef%bc%9a%e7%bc%ba%e9%99%b7%e9%a9%b1%e5%8a%a8cusb2o6%e6%8e%ba%e6%9d%82k0-5na0-5nbo3%e6%97%a0%e9%93%85%e5%8e%8b%e7%94%b5%e9%99%b6%e7%93%b7%e5%8e%8b%e7%94%b5%e5%92%8c%e9%93%81%e7%94%b5","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=95773","title":{"rendered":"J. Am. Ceram. Soc.\uff1a\u7f3a\u9677\u9a71\u52a8CuSb2O6\u63ba\u6742K0.5Na0.5NbO3\u65e0\u94c5\u538b\u7535\u9676\u74f7\u538b\u7535\u548c\u94c1\u7535\u6027\u80fd\u6f14\u53d8"},"content":{"rendered":"<p>\u3010<strong>\u5f15\u8a00<\/strong>\u3011<\/p>\n<p>\u7f3a\u9677\uff08\u6c14\u5b54\u3001\u7a7a\u4f4d\u3001\u6742\u8d28\u7b49\uff09\u5bf9\u4e8eABO<sub>3<\/sub>\u578b\u9499\u949b\u77ff\u6750\u6599\u6709\u7740\u91cd\u8981\u7684\u5f71\u54cd\u3002\u4e00\u822c\u6765\u8bb2\uff0c\u5916\u6765\u79bb\u5b50\u6216\u5316\u5408\u7269\u63ba\u6742\u4f1a\u5f62\u6210\u7279\u6b8a\u7684\u7f3a\u9677\u7ed3\u6784\uff0c\u4ece\u800c\u8c03\u63a7\u6750\u6599\u7684\u6027\u80fd\u3002\u5bf9Pb(Ti,Zr)O<sub>3<\/sub>\u57fa\u9676\u74f7\u6765\u8bf4\uff0cPb<sup>2+<\/sup> \u6216(Ti,Zr)<sup>4+<\/sup>\u88ab\u4f4e\u4ef7\u7684\u94be\u79bb\u5b50\u3001\u9530\u79bb\u5b50\u6216\u94c1\u79bb\u5b50\u53d6\u4ee3\uff0c\u5373\u53d1\u751f\u4e86\u53d7\u4e3b\u63ba\u6742\uff0c\u4e3a\u5e73\u8861\u7535\u4ef7\u4f1a\u5f62\u6210\u6c27\u7a7a\u4f4d\uff0c\u4e0e\u53d7\u4e3b\u79bb\u5b50\u5f62\u6210\u7f3a\u9677\u5076\u6781\u5b50\u3002\u8fd9\u4e9b\u7f3a\u9677\u53ef\u6709\u6548\u7a33\u5b9a\u7535\u7574\u548c\u8bf1\u5bfc\u9676\u74f7\u6027\u80fd\u201c\u786c\u5316\u201d\uff0c\u4f7f\u4e4b\u5e7f\u6cdb\u5e94\u7528\u4e8e\u9ad8\u80fd\u548c\u9ad8\u538b\u9886\u57df\u3002\u6b64\u5916\uff0c\u538b\u7535\u9676\u74f7\u7684\u5b8f\u89c2\u6027\u80fd\u4e0e\u53d7\u4e3b\u63ba\u6742\u7684\u7f3a\u9677\u5bc6\u5207\u76f8\u5173\u3002\u7136\u800c\uff0c\u53d7\u4e3b\u63ba\u6742\u540e\u9499\u949b\u77ff\u578b\u538b\u7535\u9676\u74f7\u5b8f\u89c2\u6027\u80fd\u7684\u5fae\u89c2\u673a\u5236\u5c1a\u4e0d\u6e05\u695a\u3002\u4f5c\u4e3a\u65e0\u94c5\u9676\u74f7\u7684\u5178\u578b\u4ee3\u8868\uff0c\u94cc\u9178\u94be\u94a0\uff08KNN\uff09\u57fa\u538b\u7535\u9676\u74f7\u51ed\u501f\u9ad8\u5c45\u91cc\u6e29\u5ea6 (~420<sup>o<\/sup>C)\u3001\u4f18\u5f02\u7684\u538b\u7535\u6027\u80fd\uff0c\u53d7\u5230\u4e86\u5e7f\u6cdb\u5173\u6ce8\u3002\u4e3a\u63d0\u5347KNN\u57fa\u538b\u7535\u9676\u74f7\u7684\u7535\u5b66\u6027\u80fd\uff0c\u5e38\u4e0eABO<sub>3<\/sub>\u578b\u5316\u5408\u7269\u6216\u8005\u4e0eK<sup>+<\/sup>\u3001Na<sup>+<\/sup>\u7c7b\u4f3c\u7684Li+\uff0c\u4e0eNb<sup>5+<\/sup>\u7c7b\u4f3c\u7684Ta<sup>5+<\/sup>\u3001Sb<sup>5+<\/sup>\u5f62\u6210\u56fa\u6eb6\u4f53\uff0c\u6b63\u4ea4-\u56db\u65b9\u3001\u4e09\u65b9-\u56db\u65b9\u76f8\u53d8\u901a\u5e38\u88ab\u8c03\u6574\u5230\u5ba4\u6e29\uff0c\u5f62\u6210\u591a\u6001\u76f8\u754c\u9762\u3002\u7f3a\u9677\u5bf9\u4e8e\u9499\u949b\u77ff\u538b\u7535\u9676\u74f7\u7684\u5fae\u89c2\u7ed3\u6784\u548c\u7535\u5b66\u6027\u80fd\u6709\u7740\u8f83\u5927\u5f71\u54cd\u3002\u4f46\u7f3a\u9677\u9a71\u52a8\u5b8f\u89c2\u6027\u80fd\u53d8\u5316\u7684\u5fae\u89c2\u673a\u5236\u4ecd\u6ca1\u6709\u5f97\u5230\u5b8c\u6574\u89e3\u91ca\u3002<\/p>\n<p>\u3010<strong>\u6210\u679c\u7b80\u4ecb<\/strong>\u3011<\/p>\n<p><strong>\u56db\u5ddd\u5e08\u8303\u5927\u5b66<\/strong>\u7684<strong>\u8d41\u6566\u654f\u6559\u6388\uff08\u901a\u8baf\u4f5c\u8005\uff09<\/strong>\u5728<strong>J. Am. Ceram. Soc.<\/strong>\u4e0a\u53d1\u8868\u4e86\u4e00\u7bc7\u9898\u4e3a\u201c<strong>Defect-driven evolution of piezoelectric and ferroelectric properties in CuSb<sub>2<\/sub>O<sub>6<\/sub>-doped K<sub>0.5<\/sub>Na<sub>0.5<\/sub>NbO<sub>3 <\/sub>lead-free ceramics<\/strong>\u201d\u7684\u6587\u7ae0\uff0c\u7814\u7a76\u4eba\u5458\u901a\u8fc7\u56fa\u76f8\u53cd\u5e94\u6cd5\u5236\u5907\u5f97\u5230K<sub>0.5<\/sub>Na<sub>0.5<\/sub>NbO<sub>3<\/sub> + <em>x<\/em> mol CuSb<sub>2<\/sub>O<sub>6<\/sub>\u65e0\u94c5\u538b\u7535\u9676\u74f7\uff0c\u7814\u7a76\u4e86\u5176\u538b\u7535\u548c\u94c1\u7535\u6027\u80fd\u5728\u7f3a\u9677\u9a71\u52a8\u4e0b\u7684\u6f14\u53d8\u673a\u5236\u3002CuSb<sub>2<\/sub>O<sub>6<\/sub>\u7684\u5f15\u5165\u8bf1\u5bfc\u4ea7\u751f\u4e86\u4e8c\u805a\u4f53\u7f3a\u9677\u5076\u6781\u5b50\uff08DC1\uff09\u548c\u4e09\u805a\u4f53\u7f3a\u9677\u5076\u6781\u5b50\uff08DC2\uff09\u3002\u5728\u4f4e\u63ba\u6742\u6d53\u5ea6\u4e0b\uff080.5~1.0 mol%\uff09\uff0cDC1\u548cDC2\u540c\u65f6\u5b58\u5728\uff0c\u4f7f\u9676\u74f7\u201c\u786c\u5316\u201d\uff0c\u83b7\u5f97\u4e86\u76f8\u5f53\u9ad8\u7684<em>d<\/em><sub>33<\/sub>\u503c\uff08106~126pC\/N\uff09\u3002\u8be5\u7814\u7a76\u8bf4\u660eK<sub>0.5<\/sub>Na<sub>0.5<\/sub>NbO<sub>3<\/sub>\u7684\u538b\u7535\u548c\u94c1\u7535\u6027\u80fd\u53ef\u4ee5\u901a\u8fc7\u8c03\u63a7\u6750\u6599\u7684\u7f3a\u9677\u7ed3\u6784\u6765\u5b9e\u73b0\u3002<\/p>\n<p>\u3010<strong>\u56fe\u6587\u5bfc\u8bfb<\/strong>\u3011<\/p>\n<p><strong>\u56fe1\uff1a<\/strong>KNN-<em>x<\/em>CS\u9676\u74f7\u7684XRD\u56fe\u8c31(A)\u548c\u62c9\u66fc\u5149\u8c31(B)\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-95777\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/10.1111@jace.15082-1.png\" alt=\"\" width=\"600\" height=\"789\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/10.1111@jace.15082-1.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/10.1111@jace.15082-1-228x300.png 228w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u6839\u636e\uff08A\uff09\u56fe\u53ef\u77e5\uff0cCS\u7684\u52a0\u5165\u672a\u5bfc\u81f4XRD\u56fe\u8c31\u7684\u660e\u663e\u53d8\u5316\uff0c\u6240\u6709\u7684KNN-<em>x<\/em>CS\u6837\u54c1\u5747\u4e3a\u9499\u949b\u77ff\u6b63\u4ea4\u76f8\u3002\u5f53x\u22640.015\u65f6\u65e0\u6742\u76f8\u751f\u6210\uff0c\u8bf4\u660eCS\u5df2\u7ecf\u6269\u6563\u81f3KNN\u4e2d\u5f62\u6210\u5747\u5300\u56fa\u6eb6\u4f53\u3002CS\u63ba\u6742\u6d53\u5ea6\u8fbe\u52302~2.5mol%\u65f6\u51fa\u73b0\u6742\u76f8K<sub>6<\/sub>Nb<sub>10.8<\/sub>O<sub>30<\/sub>\uff0c\u8bf4\u660eCS\u7684\u56fa\u6eb6\u9650\u4e3a2mol%\u3002\uff08B\uff09\u56fe\u4e3a\u62c9\u66fc\u632f\u52a8(<em>v<\/em><sub>1<\/sub>,<em>v<\/em><sub>2<\/sub>,<em>v<\/em><sub>3<\/sub>)\u548c(<em>v<\/em><sub>4<\/sub>,<em>v<\/em><sub>5<\/sub>)\u662fNbO<sub>6<\/sub>\u516b\u9762\u4f53\u7684\u4f38\u5c55\u6a21\u5f0f\u548c\u5f2f\u66f2\u6a21\u5f0f\u3002\u5728\u79bb\u5b50\u534a\u5f84\u8f83\u5c0f\u7684Sb<sup>5+<\/sup>\u66ff\u4ee3\u4e86Nb<sup>5+<\/sup>\uff0c\u4e14\u6c27\u7a7a\u4f4d\u751f\u6210\u7684\u7efc\u5408\u4f5c\u7528\u4e0b\uff0c\u968f<em>x<\/em>\u589e\u52a0\uff0c\u62c9\u66fc\u8f6c\u53d8<em>v<\/em><sub>1<\/sub>\u548c<em>v<\/em><sub>5<\/sub>\u51cf\u5c11\u3002<\/p>\n<p><strong>\u56fe2\uff1a<\/strong>(a-f)\u4e3aKNN-<em>x<\/em>CS\u7684X\u6ce2\u6bb5EPR\u8c31\uff1b(g)\u4e3aDC1\u548cDC2\u7684\u793a\u610f\u56fe\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-95778\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/10.1111@jace.15082-2.png\" alt=\"\" width=\"600\" height=\"621\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/10.1111@jace.15082-2.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/10.1111@jace.15082-2-290x300.png 290w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>DC1\u7684\u7535\u5076\u6781\u77e9\u6bd4DC2\u7684\u66f4\u5f3a\uff0cDC1\u66f4\u6709\u76ca\u4e8e\u9676\u74f7\u7684\u6781\u5316\uff0c\u663e\u793a\u51fa\u6bd4DC2\u66f4\u5f3a\u7684\u9489\u624e\u7535\u7574\u6548\u679c\u3002\u968f<em>x<\/em>\u7684\u589e\u52a0\uff0cDC1\u7279\u5f81\u5cf0\u7684\u5f3a\u5ea6\u9010\u6e10\u51cf\u5f31\uff0cDC2\u7684\u5f3a\u5ea6\u76f8\u5e94\u589e\u5f3a\u3002<\/p>\n<p><strong>\u56fe3\uff1a<\/strong>(a-f)\u4e3a\u5ba4\u6e29\u4e1410Hz\u6761\u4ef6\u4e0bKNN-<em>x<\/em>CS\u9676\u74f7\u7684\u7535\u538b-\u7535\u6d41\u66f2\u7ebf\u56fe\u548c\u7535\u6ede\u56de\u7ebf\uff1b(g,h)\u4e3a\u7535\u6ede\u56de\u7ebf\u6d4b\u91cf\u540e<em>P<\/em><sub>r<\/sub>\u548c<em>d<\/em><sub>33<\/sub>\u968f<em>x<\/em>\u53d8\u5316\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-95779\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/10.1111@jace.15082-3.png\" alt=\"\" width=\"600\" height=\"629\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/10.1111@jace.15082-3.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/10.1111@jace.15082-3-286x300.png 286w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u968f<em>x<\/em>\u75310.005\u589e\u52a0\u81f30.01\uff0c\u7535\u6ede\u56de\u7ebf\u9010\u6e10\u503e\u659c\u4e14\u73af\u5f62\u6709\u6240\u6536\u7f29\uff0c\u8868\u73b0\u51fa\u53cc\u7535\u6ede\u56de\u7ebf\u7684\u7279\u5f81\uff0c\u8fd9\u662f\u7531\u4e8e\u7f3a\u9677\u5076\u6781\u5b50\u5bf9\u7535\u7574\u7684\u9489\u624e\u4f5c\u7528\u6240\u81f4\u3002<\/p>\n<p><strong>\u56fe4\uff1a<\/strong>\u5ba4\u6e29\u4e1410Hz\u6761\u4ef6\u4e0b\uff0c\u6781\u5316\u540eKNN-xCS\u9676\u74f7\u7684\u7535\u538b-\u7535\u6d41\u66f2\u7ebf\u56fe\u548c\u7535\u6ede\u56de\u7ebf\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-95780\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/10.1111@jace.15082-4.png\" alt=\"\" width=\"600\" height=\"452\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/10.1111@jace.15082-4.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/10.1111@jace.15082-4-300x226.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u56fe5\uff1a<\/strong>\u6d4b\u91cf\u7ec4\u6210\u4e3a<em>x<\/em>=0\u548c<em>x<\/em>=0.01\u7684\u6781\u5316\u540e\u9676\u74f7\u7684\u7535\u6ede\u56de\u7ebf\u65f6\u7535\u7574\u8f6c\u6362\u8fc7\u7a0b\u7684\u793a\u610f\u56fe\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-95781\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/10.1111@jace.15082-5.png\" alt=\"\" width=\"600\" height=\"274\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/10.1111@jace.15082-5.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/10.1111@jace.15082-5-300x137.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u56fe6\uff1a<\/strong>(a-d)\u4e3ax=0.01\u7684\u9676\u74f7\u4e0d\u540c\u6e29\u5ea6\u4e0b\u7684\u7535\u6ede\u56de\u7ebf\u548c\u7535\u6d41-\u7535\u538b\u66f2\u7ebf\uff1b(e,f)\u4e3a<em>P<\/em><sub>r<\/sub>\u548c<em>d<\/em><sub>33<\/sub>\u968f\u6e29\u5ea6\u53d8\u5316\u60c5\u51b5\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-95774\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/10.1111@jace.15082-6.png\" alt=\"\" width=\"600\" height=\"531\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/10.1111@jace.15082-6.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/10.1111@jace.15082-6-300x266.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u53cc\u7535\u6ede\u56de\u7ebf\u968f\u6e29\u5ea6\u5347\u9ad8\u9010\u6e10\u6253\u5f00\uff0c\u5728140<sup>o<\/sup>C\u65f6\u53d8\u6210\u5355\u7535\u6ede\u56de\u7ebf\u3002\u8fd9\u8868\u660e\u9ad8\u6e29\u65f6\u7f3a\u9677\u5076\u6781\u5b50\u53ef\u4ee5\u5728\u5916\u7535\u573a\u4f5c\u7528\u4e0b\u8f7b\u6613\u8f6c\u6362\u3002\u6781\u5316\u53cd\u8f6c\u7684\u56de\u590d\u529b\u968f\u6e29\u5ea6\u5347\u9ad8\u9010\u6e10\u51cf\u5f31\uff0c\u751a\u81f3\u5728140<sup>o<\/sup>C\u65f6\u6d88\u5931\u3002<\/p>\n<p><strong>\u56fe7\uff1a<\/strong>(a-d)\u4e3a\u5ba4\u6e29\u4e0b\u4e0d\u540c\u9891\u7387\u65f6KNN-<em>x<\/em>CS\uff08<em>x<\/em>=0.01\uff09\u7684\u7535\u6ede\u56de\u7ebf\u53d8\u5316\u60c5\u51b5\uff1b(e,f)\u4e3a<em>P<\/em><sub>r<\/sub>\u548c<em>d<\/em><sub>33<\/sub>\u968f\u9891\u7387\u53d8\u5316\u60c5\u51b5\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-95775\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/10.1111@jace.15082-7.png\" alt=\"\" width=\"600\" height=\"496\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/10.1111@jace.15082-7.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/10.1111@jace.15082-7-300x248.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u968f\u6d4b\u8bd5\u9891\u7387\u753110Hz\u51cf\u5c0f\u52300.5Hz\uff0c\u9676\u74f7\u7684\u53cc\u7535\u6ede\u56de\u7ebf\u9010\u6e10\u6253\u5f00\uff0c\u57280.5Hz\u65f6\u53d8\u4e3a\u5355\u7535\u6ede\u56de\u7ebf\u3002\u9ad8\u9891\uff085-10Hz\uff09\u65f6\uff0c\u8f6c\u6362\u65f6\u95f4\u4e0d\u8db3\uff0c\u7a7a\u4f4d\u4e0d\u80fd\u8fc1\u79fb\u3002\u56e0\u6b64\uff0c\u7f3a\u9677\u5076\u6781\u5b50\u4fdd\u6301\u539f\u6765\u7684\u65b9\u5411\uff0c\u56e0\u6b64\u4ea7\u751f\u53cc\u7535\u6ede\u56de\u7ebf\u3002\u7136\u800c\uff0c\u5728\u4f4e\u9891\uff080.5Hz\uff09\uff0c\u7531\u4e8e\u6c27\u7a7a\u4f4d\u8fc1\u79fb\u7684\u65f6\u95f4\u8db3\u591f\uff0c\u7f3a\u9677\u5076\u6781\u5b50\u53ef\u4ee5\u8f6c\u5411\uff0c\u5728\u5916\u7535\u573a\u4e0b\u6781\u5316\u8f6c\u5411\uff0c\u56de\u590d\u529b\u4e0b\u964d\uff0c\u5f97\u5230\u5355\u7535\u6ede\u56de\u7ebf\u3002<\/p>\n<p><strong>\u56fe8\uff1a<\/strong>(a-f)\u4e3a\u9891\u7387\u548c\u963b\u6297( <em>Z <\/em>)\u53ca\u76f8\u4f4d\u89d2(<em>q<\/em> )\u7684\u5173\u7cfb\uff0c(g-i)\u4e3a\u6781\u5316\u540eKNN-xCS\u9676\u74f7\u7684<em>d<\/em><sub>33<\/sub>\uff0c<em>\u03b5<\/em><sub>r<\/sub>\uff0c<em>k<\/em><sub>p<\/sub>\uff0c<em>tan<\/em>\u03b4\uff0c<em>Q<\/em><sub>m<\/sub>\u53ca<em>E<\/em><sub>i<\/sub>\u968fx\u53d8\u5316\u60c5\u51b5\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-95776\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/10.1111@jace.15082-8.png\" alt=\"\" width=\"600\" height=\"391\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/10.1111@jace.15082-8.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/10.1111@jace.15082-8-300x196.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u963b\u6297\u89d2\u662f\u8bc4\u4ef7\u538b\u7535\u9676\u74f7\u7684\u6781\u5316\u6548\u7387\uff0c\u4e14\u8fbe\u5230\u7406\u60f3\u6781\u5316\u6548\u7387\u7684\u76f8\u4f4d\u89d2\u4e3a90<sup>o<\/sup>\u3002<em>x<\/em>\u75310\u589e\u957f\u52300.01\u65f6\uff0c\u76f8\u4f4d\u89d2<em>\u03b8<\/em>\u589e\u52a0\uff0c\u6781\u5316\u6548\u7387\u63d0\u9ad8\uff1b<em>x<\/em>\u8fdb\u800c\u589e\u52a0\u52300.025\u65f6\uff0c<em>\u03b8<\/em>\u4e0b\u964d\u523082.3<sup>o<\/sup>\u3002\u968f\u7740CS\u542b\u91cf\u589e\u52a0\uff0cDC1\u6548\u679c\u88ab\u524a\u5f31\uff0cDC2\u6548\u679c\u66f4\u663e\u8457\u3002\u4f7f\u5f97\u7f3a\u9677\u5076\u6781\u5b50\u5bf9\u7535\u7574\u7684\u9489\u624e\u4f5c\u7528\u51cf\u5f31\uff0c\u5728<em>x<\/em>=0.025\u65f6\uff0c\u5f97\u5230\u4e00\u4e2a\u76f8\u5bf9\u8f83\u4f4e\u7684\u673a\u68b0\u54c1\u8d28\u56e0\u6570<em>Q<\/em><sub>m<\/sub>\u4e3a206\u3002<\/p>\n<p>\u3010<strong>\u5c0f\u7ed3<\/strong>\u3011<\/p>\n<p>\u901a\u8fc7\u5408\u6210\u65e0\u94c5\u9676\u74f7K<sub>0.5<\/sub>Na<sub>0.5<\/sub>NbO<sub>3 <\/sub>+ <em>x <\/em>mol CuSb<sub>2<\/sub>O<sub>6<\/sub>\uff0c\u7814\u7a76\u4eba\u5458\u63ed\u793a\u4e86\u7f3a\u9677\u8bf1\u5bfc\u7684\u9676\u74f7\u538b\u7535\u6027\u80fd\u548c\u94c1\u7535\u6027\u80fd\u7684\u6f14\u53d8\u673a\u5236\u3002\u5b9e\u9a8c\u7ed3\u679c\u8868\u660e\u6240\u6709\u7684\u6837\u54c1\u5747\u4e3a\u6b63\u4ea4\u9499\u949b\u77ff\u76f8\u3002\u6dfb\u52a0CS\u4fc3\u8fdb\u4e86DC1\u548cDC2\u7f3a\u9677\u5076\u6781\u5b50\u7684\u5f62\u6210\u3002\u5f53<em>x<\/em>\u22640.01\u65f6\uff0c\u4e24\u79cd\u5076\u6781\u5b50\u5171\u5b58\uff0c\u4f7f\u9676\u74f7\u7684\u6027\u80fd\u786c\u5316\uff0c\u5f62\u6210\u53cc\u7535\u6ede\u56de\u7ebf\uff0c\u5728<em>x<\/em>=0.01\u65f6\u83b7\u5f97\u9ad8\u673a\u68b0\u54c1\u8d28\u56e0\u6570<em>Q<\/em><sub>m<\/sub>\u4e3a895\u3002\u5f53x\u589e\u52a0\u52300.025\u65f6\uff0cDC1\u9010\u6e10\u51cf\u5f31\uff0cDC2\u4f5c\u7528\u5f00\u59cb\u663e\u8457\uff0c\u4f7f\u5f97\u7f3a\u9677\u5076\u6781\u5b50\u5bf9\u7535\u7574\u7684\u9489\u624e\u4f5c\u7528\u51cf\u5f31\uff0c\u5728<em>x<\/em>=0.025\u65f6\uff0c\u5f97\u5230\u4e00\u4e2a\u76f8\u5bf9\u8f83\u4f4e\u7684\u673a\u68b0\u54c1\u8d28\u56e0\u6570<em>Q<\/em><sub>m<\/sub>\u4e3a206\u3002\u53ef\u4ee5\u770b\u51fa\uff0c\u5728K<sub>0.5<\/sub>Na<sub>0.5<\/sub>NbO<sub>3 <\/sub>+ <em>x <\/em>mol CuSb<sub>2<\/sub>O<sub>6<\/sub>\u9676\u74f7\u4e2d\uff0c\u538b\u7535\u6027\u80fd\u548c\u94c1\u7535\u6027\u80fd\u7684\u6f14\u53d8\u4e0e\u7f3a\u9677\u5076\u6781\u5b50DC1\u548cDC2\u5bc6\u5207\u76f8\u5173\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1a<a href=\"http:\/\/onlinelibrary.wiley.com\/doi\/10.1111\/jace.15082\/full\" target=\"_blank\" rel=\"noopener\">Defect-driven evolution of piezoelectric and ferroelectric properties in CuSb<sub>2<\/sub>O<sub>6<\/sub>-doped K<sub>0.5<\/sub>Na<sub>0.5<\/sub>NbO<sub>3<\/sub> lead-free ceramics<\/a>\uff08J. Am. Ceram. Soc., 2017, DOI: 10.1111\/jace.15082\uff09<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u65b0\u4eba\u7f16\u8f91\u90e8\u5b59\u80dc\u541b\u7f16\u8bd1\uff0c\u8d75\u98de\u9f99\u5ba1\u6838\uff0c<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\" target=\"_blank\" rel=\"noopener\">\u70b9\u6211\u52a0\u5165\u6750\u6599\u4eba\u7f16\u8f91\u90e8<\/a>\u3002<\/p>\n<p><strong>\u6750\u6599\u6d4b\u8bd5\uff0c\u6570\u636e\u5206\u6790\uff0c\u4e0a<\/strong><a href=\"http:\/\/www.ceshigu.com\/\" target=\"_blank\" rel=\"noopener\"><strong>\u6d4b\u8bd5\u8c37<\/strong><\/a><strong>\uff01<\/strong><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u7f3a\u9677\uff08\u6c14\u5b54\u3001\u7a7a\u4f4d\u3001\u6742\u8d28\u7b49\uff09\u5bf9\u4e8eABO3\u578b\u9499\u949b\u77ff\u6750\u6599\u6709\u7740\u91cd\u8981\u7684\u5f71\u54cd\u3002\u4e00\u822c\u6765\u8bb2\uff0c\u5916\u6765\u79bb\u5b50\u6216\u5316\u5408\u7269\u63ba\u6742\u4f1a\u5f62\u6210\u7279\u6b8a\u7684\u7f3a\u9677\u7ed3\u6784\uff0c\u4ece\u800c\u8c03\u63a7\u6750\u6599\u7684\u6027\u80fd\u3002\u5bf9Pb(Ti&#8230;<\/p>\n","protected":false},"author":230,"featured_media":95777,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215,2],"tags":[2135],"class_list":["post-95773","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-jiedu","category-keji","tag-2135"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/95773"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/230"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=95773"}],"version-history":[{"count":3,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/95773\/revisions"}],"predecessor-version":[{"id":95835,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/95773\/revisions\/95835"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/95777"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=95773"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=95773"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=95773"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}