{"id":95841,"date":"2017-08-11T06:31:52","date_gmt":"2017-08-10T22:31:52","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=95841"},"modified":"2017-08-11T11:04:59","modified_gmt":"2017-08-11T03:04:59","slug":"304%e5%9e%8b%e4%b8%8d%e9%94%88%e9%92%a2%e7%bd%91%e5%9f%ba%e7%94%b5%e5%88%86%e8%a7%a3%e6%b0%b4%e6%9e%90%e6%b0%a2%e3%80%81%e6%9e%90%e6%b0%a7%e5%82%ac%e5%8c%96%e7%94%b5%e6%9e%81","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=95841","title":{"rendered":"304\u578b\u4e0d\u9508\u94a2\u7f51\u57fa\u7535\u5206\u89e3\u6c34\u6790\u6c22\u3001\u6790\u6c27\u50ac\u5316\u7535\u6781\u2014\u2014\u5ec9\u4ef7\u3001\u8d28\u4f18\u3001\u6027\u80fd\u62d4\u7fa4"},"content":{"rendered":"<p><span style=\"color: #800080;\"><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/span><\/p>\n<p>\u968f\u7740\u8fd1\u5e74\u6765\u5316\u77f3\u80fd\u6e90\u7684\u65e5\u76ca\u6d88\u8017\u4ee5\u53ca\u73af\u5883\u95ee\u9898\u7684\u9010\u6e10\u6076\u5316\uff0c\u80fd\u6e90\u5371\u673a\u8feb\u5728\u7709\u776b\uff0c\u65b0\u578b\u53ef\u6301\u7eed\u80fd\u6e90\u7684\u9700\u6c42\u4e5f\u4e0e\u65e5\u4ff1\u589e\u3002\u800c\u7535\u50ac\u5316\u5206\u89e3\u6c34\u4ea7\u751f\u6c22\u6c14\u80fd\u6e90\u7684\u6280\u672f\u6709\u671b\u5e26\u9886\u4eba\u7c7b\u8d70\u51fa\u8fd9\u4e00\u56f0\u5883\u7684\u6709\u6548\u9014\u5f84\u4e4b\u4e00\u3002\u4f46\u662f\uff0c\u7531\u4e8e\u7535\u50ac\u5316\u5206\u89e3\u6c34\u6d3b\u6027\u7535\u6781\u591a\u4e3a\u8d35\u91d1\u5c5e\u6216\u8d35\u91d1\u5c5e\u6c27\u5316\u7269\uff08\u5982\u6790\u6c22\u50ac\u5316\u7535\u6781\u94c2\u548c\u6790\u6c27\u50ac\u5316\u7535\u6781\u4e8c\u6c27\u5316\u94f1\uff09\uff0c\u56e0\u800c\u5176\u5c45\u9ad8\u4e0d\u4e0b\u7684\u9020\u4ef7\u6210\u672c\u6210\u4e3a\u963b\u788d\u8fd9\u4e00\u65b0\u5174\u6280\u672f\u5927\u89c4\u6a21\u5e94\u7528\u7684\u62e6\u8def\u864e\u3002\u5982\u4f55\u5728\u4fdd\u8bc1\u7535\u6781\u6750\u6599\u5177\u5907\u9ad8\u6027\u80fd\u7684\u524d\u63d0\u4e0b\uff0c\u91c7\u7528\u5176\u4ed6\u4f4e\u5ec9\u7684\u6d3b\u6027\u7535\u6781\u662f\u5f53\u4e0b\u7535\u5206\u89e3\u6c34\u80fd\u6e90\u8f6c\u5316\u9886\u57df\u7684\u7814\u7a76\u70ed\u70b9\u4e4b\u4e00\u3002<\/p>\n<p>2017\u5e747\u67086\u65e5\uff0c\u4e2d\u5c71\u5927\u5b66\u7eaa\u7ea2\u5175\u6559\u6388\u548c\u7ae5\u53f6\u7fd4\u6559\u6388\uff08\u5171\u540c\u901a\u8baf\uff09\u8bfe\u9898\u7ec4\u5408\u4f5c\u5728<em>Advanced Materials<\/em>\u4e0a\u53d1\u8868\u4e86\u4e00\u7bc7\u9898\u4e3a\u201cCost-Effective Alkaline Water Electrolysis Based onNitrogen- and Phosphorus-Doped Self-Supportive Electrocatalysts\u201d\u7684\u8bba\u6587\uff0c\u4e3a\u7535\u89e3\u6c34\u9886\u57df\u5c55\u793a\u4e86\u4e00\u79cd\u4ee5\u5ec9\u4ef7\u7684\u4e0d\u9508\u94a2\u7f51\u884d\u751f\u51fa\u7684\u80fd\u591f\u5728\u78b1\u6027\u6761\u4ef6\u4e0b\u9ad8\u6548\u5206\u89e3\u6c34\u7684\u7535\u6781\u6750\u6599\u3002\u7814\u7a76\u4eba\u5458\u901a\u8fc7\u5c06\u666e\u901a\u5546\u7528\u7684304\u578b\u67d4\u6027\u4e0d\u9508\u94a2\u7f51\u8fdb\u884c\u9178\u8150\u8680\u5265\u79bb\u5e76\u5728\u9ad8\u6e29\u5229\u7528\u6c28\u6c14\u4ee5\u53ca\u78f7\u5316\u6c22\u6c14\u4f53\u6d3b\u5316\u5904\u7406\uff0c\u5206\u522b\u5236\u5907\u51fa\u4e86\u6027\u80fd\u5ab2\u7f8e\u91d1\u5c5e\u94c2\u548c\u6c27\u5316\u94f1\u7535\u6781\u6027\u80fd\u7684\u9633\u6781\u548c\u9634\u6781\u7535\u6781\u3002\u8fd9\u79cd\u7535\u6781\u5177\u6709\u4ee5\u4e0b\u4f18\u70b9\uff1a<\/p>\n<p><strong>\uff08<\/strong><strong>1<\/strong><strong>\uff09\u6210\u672c\u4f4e\u5ec9<\/strong>\uff1a304\u578b\u67d4\u6027\u4e0d\u9508\u94a2\u7f51\u6bcf\u5e73\u65b9\u7c73\u552e\u4ef740\u7f8e\u5143\uff0c\u800c\u5176\u4ed6\u5e38\u7528\u7684\u975e\u8d35\u91d1\u5c5e\u66ff\u4ee3\u7535\u6781\u6750\u6599\u5982\u954d\u7f51\u6bcf\u5e73\u65b9\u7c73100\u7f8e\u5143\uff0c\u78b3\u5e03\u6bcf\u5e73\u65b9\u7c73875\u7f8e\u5143\u3002\u91d1\u5c5e\u94c2\u548c\u4e8c\u6c27\u5316\u94f1\u5c31\u66f4\u52a0\u6602\u8d35\u5f97\u591a\u3002<\/p>\n<p><strong>\uff08<\/strong><strong>2<\/strong><strong>\uff09\u6d3b\u6027\u4f18\u5f02<\/strong>\uff1a\u5f97\u76ca\u4e8e\u8868\u9762\u7684\u8150\u8680\u5265\u79bb\u589e\u52a0\u7684\u6d3b\u6027\u6bd4\u8868\u9762\u79ef\u4ee5\u53ca\u9ad8\u6e29\u6c28\u6c14\u6216\u78f7\u5316\u6c22\u6c14\u4f53\u7684\u70e7\u707c\u5f15\u5165\u7684\u6c2e\u6216\u78f7\u539f\u5b50\uff0c\u5236\u5907\u7684\u6c2e\u63ba\u6742\u6d3b\u5316\u7535\u6781\u6790\u6c22\u6d3b\u6027\u4e0e\u91d1\u5c5e\u94c2\u76f8\u8fd1\uff0c\u78f7\u63ba\u6742\u6d3b\u5316\u7535\u6781\u6790\u6c27\u6d3b\u6027\u8f83\u4e8c\u6c27\u5316\u94f1\u9ad8\u3002\u7535\u89e3\u6c34\u6574\u4f53\u4f53\u7cfb\u6027\u80fd\u6bd4\u4f20\u7edf\u7ec4\u5408\u91d1\u5c5e\u94c2-\u4e8c\u6c27\u5316\u94f1\u7cfb\u7edf\u7684\u8d85\u7535\u52bf\u8fd8\u8981\u5c0f\u3002<\/p>\n<p><strong>\uff08<\/strong><strong>3<\/strong><strong>\uff09\u6027\u80fd\u7a33\u5b9a<\/strong>\uff1a\u6574\u4e2a\u4f53\u7cfb\u5c06\u8fd16\u5929\u4e0d\u95f4\u65ad\u5de5\u4f5c\u65f6\u95f4\u4e4b\u5185\u6027\u80fd\u672a\u89c2\u5bdf\u5230\u4efb\u4f55\u8870\u51cf\u3002<\/p>\n<p><span style=\"color: #800080;\"><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/span><\/p>\n<p>\uff08\u56fe\u7247\u6765\u81ea\u6587\u7ae0\u4f5c\u8005\uff09<\/p>\n<p><strong><span style=\"color: #800080;\">\u56fe\u4e00\uff1a\u9633\u6781\u4e0d\u9508\u94a2\u7f51\u7684\u5904\u7406\u65b9\u6cd5\u793a\u610f\u56fe\u53ca\u5904\u7406\u524d\u540e\u4e0d\u9508\u94a2\u7f51\u7684\u5f62\u8c8c\u3001\u7ec4\u6210\u5206\u6790<\/span><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-95842 \" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/1-23.jpg\" alt=\"\" width=\"594\" height=\"281\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/1-23.jpg 1429w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/1-23-300x142.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/1-23-768x363.jpg 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/1-23-1024x484.jpg 1024w\" sizes=\"(max-width: 594px) 100vw, 594px\" \/><\/p>\n<p>\uff08a\uff09\u9633\u6781\u4e0d\u9508\u94a2\u7f51\u7684\u6c34\u70ed\u5265\u79bb\u4ee5\u53ca\u6c2e\u63ba\u6742\u5904\u7406\u65b9\u6cd5\u793a\u610f\u56fe\uff1bSS\uff1a\u672a\u5904\u7406\u7684\u4e0d\u9508\u94a2\u7f51\uff0cESS\uff1a\u5265\u79bb\u8150\u8680\u540e\u7684\u4e0d\u9508\u94a2\u7f51\uff0cNESS\uff1a\u6c2e\u63ba\u6742\u53ca\u5265\u79bb\u8150\u8680\u540e\u7684\u4e0d\u9508\u94a2\u7f51<\/p>\n<p>\uff08b-c\uff09\u5904\u7406\u524d\u3001\u540e\u7684\u626b\u63cf\u7535\u955c\u56fe\uff08SEM\uff09\uff1b\u7ecf\u8fc7\u5904\u7406\u540e\uff0c\u5728\u4e0d\u9508\u94a2\u7f51\u7ea4\u7ef4\u8868\u9762\u53d8\u5f97\u7c97\u7cd9\uff0c\u4e14\u51fa\u73b0\u7ec6\u5fae\u7684\u7eb3\u7c73\u9897\u7c92\u3002\u56e0\u6b64\u5904\u7406\u540e\u4e0d\u9508\u94a2\u7f51\u6bd4\u8868\u9762\u79ef\u7684\u589e\u5927\uff0c\u4f7f\u5f97\u6d3b\u6027\u4f4d\u70b9\u7684\u589e\u591a\uff1b<\/p>\n<p>\uff08d\uff09\u80fd\u8c31\u5143\u7d20\u5206\u5e03\u56fe\uff1b\u7ecf\u8fc7\u6c2e\u5316\u5904\u7406\u540e\uff0c\u5728\u4e0d\u9508\u94a2\u7535\u6781\u5185\u90e8\u5f15\u5165N\u539f\u5b50\u3002<\/p>\n<p><strong><span style=\"color: #800080;\">\u56fe\u4e8c\uff1a\u5904\u7406\u540e\u7535\u6781\u7684\u7269\u76f8\u7ec4\u6210\u53ca\u5143\u7d20\u4ef7\u6001\u5206\u6790<\/span><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-95843 \" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/2-25.jpg\" alt=\"\" width=\"597\" height=\"381\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/2-25.jpg 1429w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/2-25-300x192.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/2-25-768x491.jpg 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/2-25-1024x654.jpg 1024w\" sizes=\"(max-width: 597px) 100vw, 597px\" \/><\/p>\n<p>\uff08a\uff09\u5904\u7406\u540e\u7535\u6781\u7684X\u5c04\u7ebf\u884d\u5c04\u56fe\uff08XRD\uff09\uff1b\u7531\u56fe\u4e2d\u5cf0\u4f4d\u7f6e\u53ca\u5f3a\u5ea6\u7684\u504f\u79fb\uff0c\u80fd\u591f\u770b\u51fa\u7ecf\u8fc7\u5265\u79bb\u548c\u6c2e\u63ba\u6742\u540e\uff0c\u4e0d\u9508\u94a2\u7535\u6781\u7684\u6676\u578b\u7ed3\u6784\u53d1\u751f\u4e86\u6539\u53d8\u3002<\/p>\n<p>\uff08b-d\uff09\u5904\u7406\u540e\u7535\u6781\u7684X\u5c04\u7ebf\u7535\u5b50\u80fd\u8c31\uff08XPS\uff09\u5206\u6790\u56fe\uff1b\u7ecf\u8fc7\u5904\u7406\u540e\uff0c\u5728\u4e0d\u9508\u94a2\u6750\u6599\u4e2d\u89c2\u6d4b\u5230\u4e86\u5421\u5576\u6c2e\u548c\u5421\u54af\u6c2e\u4e24\u79cd\u6c2e\u7ec4\u6210\u7684\u5b58\u5728\u3002\u5176\u4e2d\u5421\u5576\u6c2e\u88ab\u62a5\u9053\u6709\u50ac\u5316\u5206\u89e3\u6c34\u7684\u6d3b\u6027\u3002\u540c\u65f6\uff0cFe\u5143\u7d20\u548cCr\u5143\u7d20\uff08\u4e8c\u8005\u5747\u662f\u4e0d\u9508\u94a2\u7f51\u7684\u7ec4\u6210\u5143\u7d20\uff09\u5411\u4f4e\u4ef7\u4f4d\u7f6e\u504f\u79fb\uff0c\u8bc1\u660e\u4e86\u4f4e\u4ef7\u91d1\u5c5e\u7684\u4ea7\u751f\u3002<\/p>\n<p><strong><span style=\"color: #800080;\">\u56fe\u4e09\uff1a\u9633\u6781\u4e0d\u9508\u94a2\u7f51\u7684\u7535\u5316\u5b66\u6027\u80fd\u8868\u5f81\u5206\u6790\u3002<\/span><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-95844 \" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/3-20.jpg\" alt=\"\" width=\"598\" height=\"465\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/3-20.jpg 1431w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/3-20-300x233.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/3-20-768x597.jpg 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/3-20-1024x796.jpg 1024w\" sizes=\"(max-width: 598px) 100vw, 598px\" \/><\/p>\n<p>\uff08a-c\uff09\u5404\u6837\u54c1\u7684\u7ebf\u626b\u66f2\u7ebf\u3001\u5854\u83f2\u5c14\u66f2\u7ebf\u6d4b\u8bd5\u4ee5\u53ca\u5948\u594e\u65af\u7279\uff08Nyquist\uff09\u66f2\u7ebf\uff1b\u5176\u4e2d\u5904\u7406\u540e\u7684\u9633\u6781\u4e0d\u9508\u94a2\u7f51\u5c55\u73b0\u51fa\u4f18\u5f02\u7684\u6790\u6c27\u6027\u80fd\u548c\u7535\u5b66\u6027\u80fd\uff1bIrO<sub>2<\/sub>-CC\uff1a\u9644\u7740\u5728\u78b3\u5e03\u4e0a\u7684\u4e8c\u6c27\u5316\u94f1\uff0c\u5bf9\u7167\u7ec4<\/p>\n<p>\uff08d\uff09\u7a33\u5b9a\u6027\u6d4b\u8bd5\u4e2d\u6c27\u6c14\u4ea7\u91cf\u548c\u7535\u6d41\u6d4b\u8bd5\u56fe\uff1b<\/p>\n<p>\uff08e\uff09\u6052\u7535\u4f4d\uff086\u5929\uff09\u548c\u6052\u7535\u6d41\uff085.6\u5929\uff09\u6761\u4ef6\u4e0b\u7535\u6781\u7684\u7a33\u5b9a\u6027\u6027\u80fd\uff1b<\/p>\n<p>\uff08f-i\uff09\u957f\u65f6\u95f4\u7a33\u5b9a\u6027\u6d4b\u8bd5\u540e\u7684\u6750\u6599\u6676\u578b\u5f62\u8c8c\u7ed3\u6784\u4ee5\u53ca\u5143\u7d20\u4ef7\u6001\u7684\u5206\u6790\u8868\u5f81\uff1b\u7ecf\u8fc7\u7a33\u5b9a\u6027\u6027\u80fd\u6d4b\u8bd5\u540e\uff0c\u7535\u6781\u6750\u6599\u7684\u5f62\u8c8c\u548c\u5143\u7d20\u4ef7\u6001\u51e0\u4e4e\u672a\u53d1\u751f\u4efb\u4f55\u6539\u53d8\u3002<\/p>\n<p><strong><span style=\"color: #800080;\">\u56fe\u56db\uff1a\u9634\u6781\u4e0d\u9508\u94a2\u7535\u6781\u7684\u5236\u5907\u548c\u8868\u5f81<\/span><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-95845 \" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/4-18.jpg\" alt=\"\" width=\"597\" height=\"480\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/4-18.jpg 1429w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/4-18-300x241.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/4-18-768x617.jpg 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/4-18-1024x823.jpg 1024w\" sizes=\"(max-width: 597px) 100vw, 597px\" \/><\/p>\n<p>\uff08a\uff09\u9634\u6781\u4e0d\u9508\u94a2\u7f51\u7684\u6c2e\u3001\u78f7\u63ba\u6742\u5904\u7406\u65b9\u6cd5\u793a\u610f\u56fe\uff1bNESSP\uff1a\u6c2e\u548c\u78f7\u53cc\u63ba\u6742\u7684\u5265\u79bb\u8150\u8680\u4e0d\u9508\u94a2\u7f51<\/p>\n<p>\uff08b-d\uff09\u7ecf\u8fc7\u78f7\u63ba\u6742\u540e\u7535\u6781\u6750\u6599\u7684XRD\u4ee5\u53caXPS\u8868\u5f81\u6d4b\u8bd5\u56fe\uff1b\u5728\u8fdb\u884c\u78f7\u539f\u5b50\u7684\u63ba\u6742\u5f15\u5165\u8fc7\u7a0b\u4e2d\uff0c\u53d1\u73b0\u4e86FeP\u7ec4\u5206\u7684\u5b58\u5728\uff0cXPS\u4e5f\u5bf9Fe-P\u7684\u5b58\u5728\u8fdb\u884c\u4e86\u8fdb\u4e00\u6b65\u7684\u8bc1\u660e\u3002<\/p>\n<p>\uff08e-g\uff09\u5404\u5bf9\u7167\u6837\u54c1\u53ca\u5904\u7406\u6837\u54c1\u7684\u7535\u5b66\u6027\u80fd\u8868\u5f81\uff1a\u7ebf\u626b\u66f2\u7ebf\u3001\u5854\u83f2\u5c14\u66f2\u7ebf\u6d4b\u8bd5\uff1bSS\uff1a\u672a\u5904\u7406\u7684\u578b\u4e0d\u9508\u94a2\u7f51\uff1bSSP\uff1a\u4ec5\u78f7\u63ba\u6742\u7684\u672a\u5265\u79bb\u4e0d\u9508\u94a2\u7f51\uff0cPt-mesh\uff1a\u91d1\u5c5e\u94c2\u7f51\uff0c\u5bf9\u7167\u7ec4\u3002<\/p>\n<p>\uff08h-i\uff09\u9634\u6781\u4e0d\u9508\u94a2\u7535\u6781\u7a33\u5b9a\u6027\u6d4b\u8bd5\u3002<\/p>\n<p><strong><span style=\"color: #800080;\">\u56fe\u4e94\uff1a\u4e0d\u9508\u94a2\u9634\u6781\u3001\u9633\u6781\u7ec4\u5408\u7535\u5206\u89e3\u6c34\u80fd\u6e90\u8f6c\u5316\u88c5\u7f6e\u6027\u80fd<\/span><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-95846 \" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/5-13.jpg\" alt=\"\" width=\"596\" height=\"368\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/5-13.jpg 1429w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/5-13-300x185.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/5-13-768x474.jpg 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/5-13-1024x632.jpg 1024w\" sizes=\"(max-width: 596px) 100vw, 596px\" \/><\/p>\n<p>\uff08a-c\uff09\u88c5\u7f6e\u793a\u610f\u56fe\u53ca\u7ebf\u626b\u66f2\u7ebf\uff1b<\/p>\n<p>\uff08d\uff09\u5404\u6837\u54c1\u5173\u952e\u50ac\u5316\u6027\u80fd\u6307\u6807\u5bf9\u6bd4\uff1b\u5904\u7406\u540e\u7684\u4e0d\u9508\u94a2\u7535\u5206\u89e3\u6c34\u80fd\u6e90\u8f6c\u5316\u88c5\u7f6e\u6027\u80fd\u6781\u5176\u4f18\u5f02\uff0c\u5728\u9ad8\u7535\u6d41\u6761\u4ef6\u4e0b\uff0c\u751a\u81f3\u6bd4\u8d35\u91d1\u5c5e\u7cfb\u7edf\u5177\u6709\u66f4\u5c0f\u7684\u8fc7\u7535\u4f4d\u3002<\/p>\n<p>\uff08e-f\uff095.6\u5929\u7684\u88c5\u7f6e\u7a33\u5b9a\u6027\u6d4b\u8bd5\u3002<\/p>\n<p><span style=\"color: #800080;\"><strong>\u3010\u7ed3\u8bba\u3011<\/strong><\/span><\/p>\n<p>\u672c\u6587\u62a5\u9053\u4e86\u4e00\u79cd\u4ee5304\u578b\u4e0d\u9508\u94a2\u7f51\u4e3a\u539f\u6750\u6599\uff0c\u5236\u5907\u5177\u6709\u9ad8\u6bd4\u8868\u9762\u79ef\u548c\u6c2e\u6216\u78f7\u539f\u5b50\u63ba\u6742\u7684\u7535\u5206\u89e3\u6c34\u50ac\u5316\u7535\u6781\u7684\u65b9\u6cd5\u3002\u8be5\u5de5\u4f5c\u7cfb\u7edf\u5730\u7814\u7a76\u4e86\u5265\u79bb\u8150\u8680\u4ee5\u53ca\u6c2e\u3001\u78f7\u539f\u5b50\u7684\u5b58\u5728\u5bf9\u6837\u54c1\u7535\u5316\u5b66\u6790\u6c22\u6790\u6c27\u6027\u80fd\u6240\u9020\u6210\u7684\u5f71\u54cd\uff0c\u5e76\u5bf9\u5176\u4e2d\u5404\u6837\u54c1\u7684\u7269\u76f8\u7ec4\u6210\u8fdb\u884c\u4e86\u6df1\u5165\u7684\u5206\u6790\uff0c\u4ece\u800c\u6210\u529f\u7684\u8bbe\u8ba1\u7ec4\u88c5\u51fa\u4e86\u5177\u5907\u5ab2\u7f8e\u8d35\u91d1\u5c5e\u6216\u8d35\u91d1\u5c5e\u6c27\u5316\u7269\u7684\u80fd\u7684\u7535\u5206\u89e3\u6c34\u80fd\u6e90\u8f6c\u5316\u88c5\u7f6e\u3002\u6240\u5236\u5907\u7684\u7535\u6781\u540c\u65f6\u5177\u6709\u4ef7\u683c\u4f4e\u5ec9\uff0c\u6027\u80fd\u7a33\u5b9a\u7684\u7279\u70b9\u3002\u672c\u5de5\u4f5c\u53ef\u4e3a\u7535\u5206\u89e3\u6c34\u7814\u7a76\u9886\u57df\u7684\u79d1\u7814\u5de5\u4f5c\u8005\u53c2\u8003\uff0c\u63a8\u8fdb\u7535\u89e3\u6c34\u80fd\u6e90\u8f6c\u5316\u6280\u672f\u7684\u5e94\u7528\u3002<\/p>\n<p><span style=\"color: #800080;\"><strong>\u3010\u6587\u7ae0\u94fe\u63a5\u3011<\/strong><\/span><\/p>\n<p>Balogun M. et al. Cost-Effective Alkaline Water Electrolysis Based onNitrogen- and Phosphorus-Doped Self-Supportive Electrocatalysts, <em>Adv. Mater.<\/em>, 2017, <a href=\"http:\/\/onlinelibrary.wiley.com\/doi\/10.1002\/adma.201702095\/abstract\">DOI: 10.1002\/adma.201702095<\/a><\/p>\n<p><span style=\"color: #800080;\"><strong>\u3010\u901a\u8baf\u4f5c\u8005\u7b80\u4ecb\u3011<\/strong><\/span><\/p>\n<p><strong>\u7eaa\u7ea2\u5175<\/strong>\u6559\u6388\uff1ahttp:\/\/ce.sysu.edu.cn\/\/Item\/7898.aspx<\/p>\n<p>\u5de5\u5b66\u535a\u58eb\uff0c\u4e2d\u5c71\u5927\u5b66\u5316\u5b66\u4e0e\u5316\u5b66\u5de5\u7a0b\u5b66\u9662\u6559\u6388\uff0c\u535a\u58eb\u751f\u5bfc\u5e08\uff0c\u957f\u6c5f\u5b66\u8005\uff0c\u56fd\u5bb6\u6770\u51fa\u9752\u5e74\u79d1\u5b66\u57fa\u91d1\u83b7\u5f97\u8005\uff0c\u79d1\u6280\u90e8\u4e2d\u9752\u5e74\u79d1\u6280\u521b\u65b0\u9886\u519b\u4eba\u624d\uff0c\u5e7f\u4e1c\u7701\u201c\u73e0\u6c5f\u5b66\u8005\u201d\u7279\u8058\u6559\u6388\uff0c\u4e2d\u5c71\u5927\u5b66\u7cbe\u7ec6\u5316\u5de5\u7814\u7a76\u9662\u9662\u957f\u3001\u4e2d\u5c71\u5927\u5b66\u60e0\u5dde\u7814\u7a76\u9662\u9662\u957f\u3002\u7814\u7a76\u65b9\u5411\u4e3a\u73af\u5883\u53cb\u597d\u7684\u50ac\u5316\u8fc7\u7a0b(\u591a\/\u5747\u76f8\u50ac\u5316\u3001\u4eff\u751f\u50ac\u5316\u548c\u73af\u5883\u50ac\u5316)\uff0c\u7cbe\u7ec6\u5316\u5de5\u3001\u5929\u7136\u7cbe\u7ec6\u5316\u5b66\u54c1\u7684\u5206\u79bb\u4e0e\u5408\u6210\uff0c\u7eff\u8272\u5316\u5de5\u8fc7\u7a0b\uff0c\u5316\u5de5\u56ed\u533a\u7ba1\u7406\u3002<\/p>\n<p><strong>\u7ae5\u53f6\u7fd4<\/strong>\u6559\u6388\uff1ahttp:\/\/ce.sysu.edu.cn\/\/Item\/7921.aspx<\/p>\n<p>\u4e2d\u5c71\u5927\u5b66\u5316\u5b66\u5b66\u9662\u6559\u6388\uff0c\u535a\u58eb\u751f\u5bfc\u5e08\u3002\u517c\u4efb\u5e7f\u4e1c\u7701\u8868\u9762\u5de5\u7a0b\u534f\u4f1a\u7406\u4e8b\u548c\u5e7f\u5dde\u5e02\u7535\u9540\u534f\u4f1a\u7406\u4e8b\uff0c\u4e2d\u56fd\u5316\u5b66\u4f1a\u5316\u5b66\u6559\u80b2\u59d4\u5458\u4f1a\u59d4\u5458\uff0c\u300a\u5927\u5b66\u5316\u5b66\u300b\u7f16\u59d4\uff0c\u5e7f\u4e1c\u7701\u7a00\u571f\u534f\u4f1a\u7406\u4e8b\uff0c\u4e2d\u56fd\u6709\u8272\u91d1\u5c5e\u5b66\u4f1a\u51b6\u91d1\u7269\u7406\u5316\u5b66\u5b66\u672f\u59d4\u5458\u4f1a\u59d4\u5458\uff0c\u4e2d\u56fd\u5316\u5b66\u4f1a\u7535\u5316\u5b66\u4e13\u4e1a\u59d4\u5458\u4f1a\u59d4\u5458\uff0c\u5e7f\u4e1c\u7701\u5316\u5b66\u4f1a\u79d8\u4e66\u957f\u3002\u76ee\u524d\u4e3b\u8981\u7814\u7a76\u65b9\u5411\u4e3a\u7eb3\u7c73\u80fd\u6e90\u6750\u6599\u4e0e\u65b0\u80fd\u6e90\u5668\u4ef6\uff0c\u4e3b\u8981\u5305\u62ec\u7eb3\u7c73\u8fc7\u6e21\u91d1\u5c5e\u6c27\u5316\u7269\u3001\u7eb3\u7c73\u534a\u5bfc\u4f53\u6750\u6599\u3001\u5149\u50ac\u5316\u548c\u7535\u50ac\u5316\u6750\u6599\u3001\u5149\u7535\u5316\u5b66\u3001\u8d85\u7ea7\u7535\u5bb9\u5668\u548c\u9502\u79bb\u5b50\u7535\u6c60\u7b49\u3002<\/p>\n<p>\u672c\u5bfc\u8bfb\u7531\u8bba\u6587\u4f5c\u8005\u8bfe\u9898\u7ec4\u674e\u660e\u9633\u4f9b\u7a3f\uff0c\u6750\u6599\u4eba\u7279\u9080\u7f16\u8f91\u5218\u7530\u5b87\u7f16\u8f91\u5ba1\u9605\u540e\u53d1\u8868\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u968f\u7740\u8fd1\u5e74\u6765\u5316\u77f3\u80fd\u6e90\u7684\u65e5\u76ca\u6d88\u8017\u4ee5\u53ca\u73af\u5883\u95ee\u9898\u7684\u9010\u6e10\u6076\u5316\uff0c\u80fd\u6e90\u5371\u673a\u8feb\u5728\u7709\u776b\uff0c\u65b0\u578b\u53ef\u6301\u7eed\u80fd\u6e90\u7684\u9700\u6c42\u4e5f\u4e0e\u65e5\u4ff1\u589e\u3002\u800c\u7535\u50ac\u5316\u5206\u89e3\u6c34\u4ea7\u751f\u6c22\u6c14\u80fd\u6e90\u7684\u6280\u672f\u6709\u671b\u5e26\u9886\u4eba\u7c7b\u8d70\u51fa&#8230;<\/p>\n","protected":false},"author":2791,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[],"class_list":["post-95841","post","type-post","status-publish","format-standard","hentry","category-jiedu"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/95841"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/2791"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=95841"}],"version-history":[{"count":2,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/95841\/revisions"}],"predecessor-version":[{"id":95848,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/95841\/revisions\/95848"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=95841"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=95841"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=95841"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}