{"id":97199,"date":"2017-08-20T06:30:03","date_gmt":"2017-08-19T22:30:03","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=97199"},"modified":"2017-08-19T22:09:30","modified_gmt":"2017-08-19T14:09:30","slug":"%e6%96%b0%e5%8a%a0%e5%9d%a1%e5%8d%97%e6%b4%8b%e7%90%86%e5%b7%a5%e5%be%90%e6%a2%bd%e5%b7%9d%e6%95%99%e6%8e%88%e8%af%be%e9%a2%98%e7%bb%84-advanced-energy-materials%ef%bc%9a%e5%a4%9a%e4%bd%8d%e7%82%b9","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=97199","title":{"rendered":"\u65b0\u52a0\u5761\u5357\u6d0b\u7406\u5de5\u5f90\u68bd\u5ddd\u6559\u6388\u8bfe\u9898\u7ec4 Advanced Energy Materials\uff1a\u591a\u4f4d\u70b9\u7b56\u7565\u6539\u6027\u7eb3\u7c73\u94af\u9897\u7c92\u8868\u9762\u4ee5\u63d0\u5347\u5176\u78b1\u6027\u73af\u5883\u4e0b\u7684\u6790\u6c22\u53cd\u5e94\u6d3b\u6027"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/p>\n<p>\u6790\u6c22\u53cd\u5e94\uff08HER\uff09\u662f\u6c34\u7535\u89e3\u7684\u9634\u6781\u53cd\u5e94\uff0c\u540c\u65f6\u4e5f\u662f\u4e00\u79cd\u7b80\u5355\u3001\u9ad8\u6548\u7684\u5236\u6c22\u65b9\u6cd5\u3002\u5de5\u4e1a\u6c34\u7535\u89e3\u5236\u6c22\u901a\u5e38\u662f\u572825\u201335% KOH\u78b1\u6027\u7535\u89e3\u6db2\u4e2d\u8fdb\u884c\u3002\u7136\u800c\uff0c\u7531\u4e8e\u78b1\u6027\u4ecb\u8d28\u6240\u63d0\u4f9b\u7684\u8d28\u5b50\uff08H<sup>+<\/sup>\uff09\u6d53\u5ea6\u6709\u9650\uff0c\u53d1\u751f\u5728\u8d35\u91d1\u5c5e\u8868\u9762\u7684\u6790\u6c22\u53cd\u5e94\u5f80\u5f80\u4f1a\u6bd4\u9178\u6027\u4ecb\u8d28\u6761\u4ef6\u4e0b\u6162\u51e0\u4e2a\u6570\u91cf\u7ea7\u3002\u672c\u8d28\u4e0a\u53ef\u4ee5\u5c06\u78b1\u6027\u6761\u4ef6\u4e0bHER\u8fc7\u7a0b\u770b\u4f5c\u662f\u4e24\u4e2a\u8fde\u7eed\u7684\u6b65\u9aa4\uff1a1. \u6c34\u5206\u5b50\u7684\u5171\u4ef7\u952e\u88ab\u6253\u65ad\uff0c\u89e3\u79bb\u4ea7\u751fH<sup>+<\/sup>\uff1b2. \u5438\u9644\u5728\u8d35\u91d1\u5c5e\u8868\u9762\u7684H<sup>+<\/sup>\u91cd\u7ec4\u590d\u5408\u5f62\u6210H<sub>2<\/sub>\u3002\u6b63\u662f\u7531\u4e8e\u7b2c\u4e00\u6b65\u6253\u7834\u6c34\u5206\u5b50H-O\u952e\u7684\u7f13\u6162\u52a8\u529b\u5b66\u8fc7\u7a0b\u4f7f\u5f97\u5b83\u6210\u4e3a\u78b1\u6027\u6761\u4ef6\u4e0b\u8d35\u91d1\u5c5eHER\u50ac\u5316\u7684\u9650\u901f\u6b65\u9aa4\u3002\u4e3a\u4e86\u63d0\u5347\u6574\u4f53\u53cd\u5e94\u7684\u901f\u5ea6\uff0c\u5219\u9700\u8981\u5728\u8d35\u91d1\u5c5e\u8868\u9762\u52a0\u5165\u989d\u5916\u7684\u6c34\u89e3\u79bb\u50ac\u5316\u4f4d\u70b9\uff0c\u7528\u4ee5\u52a0\u901f\u4ea7\u751f\u8d28\u5b50\uff0c\u63d0\u9ad8\u5c40\u90e8\u7684\u8d28\u5b50\u4f9b\u7ed9\u901f\u5ea6\uff0c\u4ece\u800c\u7f13\u89e3\u8d28\u5b50\u7a00\u7f3a\u5e26\u6765\u7684\u5f71\u54cd\u3002\u57fa\u4e8e\u8fd9\u79cd\u673a\u5236\uff0c\u5df2\u7ecf\u6709\u4e00\u4e9b\u76f8\u5173\u7684\u62a5\u9053\uff0c\u4f8b\u5982\u5728\u91d1\u5c5e\uff08Fe\u3001Co\u3001Ni\uff09\u6c27\u6c27\u6c22\u5316\u5408\u7269\u4fee\u9970\u7684\u5757\u4f53Pt\uff08111\uff09\u8868\u9762\uff0c\u91d1\u5c5e\u6c27\u6c27\u6c22\u5316\u5408\u7269\u7684\u786e\u53ef\u4ee5\u4fc3\u8fdb\u78b1\u6027\u6761\u4ef6\u4e0b\u6c34\u7684\u89e3\u79bb\uff0c\u4ece\u800c\u63d0\u9ad8Pt\uff08111\uff09\u9762\u7684HER\u50ac\u5316\u6027\u80fd\u3002\u7136\u800c\uff0c\u7531\u4e8e\u7eb3\u7c73\u6750\u6599\u8868\u9762\u4fee\u9970\u7684\u6280\u672f\u9650\u5236\uff0c\u8fd9\u4e9b\u7814\u7a76\u76ee\u524d\u53ea\u5c40\u9650\u4e8e\u5757\u4f53\u8d35\u91d1\u5c5e\u8868\u9762\uff0c\u5e76\u6ca1\u6709\u4f53\u73b0\u51fa\u8f83\u9ad8\u7684\u5b9e\u9645\u5e94\u7528\u4ef7\u503c\u3002\u5982\u4f55\u7528\u91d1\u5c5e\uff08Fe\u3001Co\u3001Ni\uff09\u6c27\u6c27\u6c22\u5316\u5408\u7269\u4fee\u9970\u7eb3\u7c73\u6750\u6599\u5c24\u5176\u662f\u7eb3\u7c73\u9897\u7c92\u7684\u8868\u9762\u5c06\u4f1a\u662f\u4e00\u4e2a\u4e0d\u5c0f\u7684\u6311\u6218\u3002\u4e0d\u4ec5\u5982\u6b64\uff0c\u66f4\u52a0\u7ec6\u5206\u6765\u770b\uff0c\u66f4\u7cbe\u786e\u5730\u8c03\u63a7\u7eb3\u7c73\u9897\u7c92\u8868\u9762\u4e0a\u4e24\u79cd\u50ac\u5316\u53cd\u5e94\u4f4d\u70b9\u7684\u8986\u76d6\u6bd4\u4f8b\uff0c\u5bfb\u627e\u4e00\u4e2a\u5e73\u8861\u7684\u3001\u6700\u4f18\u7684\u8986\u76d6\u7387\u4ee5\u63d0\u5347HER\u6574\u4f53\u6d3b\u6027\u8fbe\u5230\u6700\u9ad8\u4e5f\u540c\u6837\u662f\u76ee\u524d\u9762\u4e34\u7684\u4e00\u4e2a\u95ee\u9898\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c\u65b0\u52a0\u5761\u5357\u6d0b\u7406\u5de5\u5927\u5b66\u6750\u6599\u79d1\u5b66\u5de5\u7a0b\u5b66\u9662\u5f90\u68bd\u5ddd\u6559\u6388\u8bfe\u9898\u7ec4\u7814\u7a76\u62a5\u544a\u4e86\u4e00\u79cd\u201c\u81ea\u4e0a\u800c\u4e0b\u201d\u7684\u5408\u6210\u7b56\u7565\uff0c\u4ee5Pd\/Fe<sub>3<\/sub>O<sub>4<\/sub>\u6838\u58f3\u7eb3\u7c73\u9897\u7c92\u4e3a\u8d77\u59cb\u7eb3\u7c73\u6750\u6599\uff0c\u5229\u7528\u7535\u5316\u5b66\u5faa\u73af\u8150\u8680\u7684\u65b9\u6cd5\u7cbe\u7ec6\u53ef\u63a7\u5730\u8c03\u8282FeO<sub>x<\/sub>(OH)<sub>2\u22122x<\/sub>\u5728\u7eb3\u7c73Pd\u8868\u9762\u7684\u8986\u76d6\u7387\u3002\u539f\u4f4d\u540c\u6b65\u8f90\u5c04\uff08XAS\uff09\u4ee5\u53ca\u7535\u5316\u5b66CV\u8868\u5f81\u6570\u636e\u8868\u660e\u968f\u7740\u7535\u5316\u5b66\u5faa\u73af\u8150\u8680\u7684\u5708\u6570\u589e\u52a0\uff0cFeO<sub>x<\/sub>(OH)<sub>2\u22122x<\/sub>\u7684\u8986\u76d6\u7387\u5448\u73b0\u51fa\u5148\u5feb\u901f\u518d\u5e73\u7f13\u7684\u51cf\u5c11\u8d8b\u52bf\uff0c\u800cFe\u6574\u4f53\u4ef7\u6001\u5448\u73b0\u51fa\u201cV\u201d\u578b\u8d8b\u52bf\u2014\u2014\u5148\u964d\u540e\u5347\uff0c\u8fd9\u4e0e\u9884\u671f\u76f8\u543b\u5408\u3002HER\u7535\u5316\u5b66\u6d3b\u6027\u8868\u5f81\u7ed3\u679c\u8868\u660e\uff0cPd\/FeO<sub>x<\/sub>(OH)<sub>2\u22122x<\/sub>\u7eb3\u7c73\u7c92\u5b50\u5728\u78b1\u6027\u6761\u4ef6\u4e0b\u7684HER\u6d3b\u52a8\u4e0e\u8868\u9762Fe(OH)<sub>2\u22122x<\/sub>\u8986\u76d6\u7387\u5448\u73b0\u51fa\u706b\u5c71\u5f62\u72b6\u7684\u5173\u7cfb\u3002FeO<sub>x<\/sub>(OH)<sub>2\u22122x<\/sub>\u8986\u76d6\u7387\u572840%\u5de6\u53f3\u5c55\u73b0\u51fa\u6700\u4f18\u7684HER\u78b1\u6027\u50ac\u5316\u6027\u80fd\uff0c\u5176\u5185\u5728\u6d3b\u6027\u662f\u7eafPd\u7eb3\u7c73\u9897\u7c92\u768419\u500d\u3002FeO<sub>x<\/sub>(OH)<sub>2\u22122x<\/sub>\u4f4d\u70b9\u7684\u589e\u591a\u4f1a\u63d0\u5347\u6c34\u89e3\u79bb\u7684\u91cf\uff0c\u4e3a\u76f8\u90bb\u7684Pd\u4f4d\u70b9\u63d0\u4f9b\u66f4\u591a\u7684H<sup>+<\/sup>\uff0c\u4f46\u4e0e\u6b64\u540c\u65f6\u53c8\u4f1a\u4f7fPd\u7684\u6d3b\u6027\u4f4d\u70b9\u6570\u91cf\u51cf\u5c11\uff0c\u6b63\u662f\u8fd9\u79cd\u7ade\u4e89\u5173\u7cfb\u4f7f\u5f97HER\u6d3b\u6027\u5448\u73b0\u51fa\u5148\u5347\u540e\u964d\u7684\u89c4\u5f8b\u3002\u76f8\u5173\u7ed3\u679c\u4ee5\u201cA Multisite Strategy for Enhancing the Hydrogen Evolution Reaction on a Nano-Pd Surface in Alkaline Media\u201d\u4e3a\u9898\uff0c\u53d1\u8868\u5728 Advanced Energy Materials \uff08DOI: 10.1002\/aenm.201701129\uff09\u4e0a\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p>\u56fe\u4e00\uff1aPd\/Fe<sub>3<\/sub>O<sub>4<\/sub>\u6838\u58f3\u7eb3\u7c73\u9897\u7c92\u7684\u7535\u955c\u7167\u7247\u53ca\u540c\u6b65\u8f90\u5c04\u56fe\u8c31\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-97208 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/1-49.jpg\" alt=\"\" width=\"600\" height=\"555\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/1-49.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/1-49-300x278.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09Pd \u7eb3\u7c73\u9897\u7c92\u7684\u7535\u955c\u7167\u7247\uff1b<\/p>\n<p>\uff08b\uff09Pd\/Fe<sub>3<\/sub>O<sub>4<\/sub> \u6838\u58f3\u7eb3\u7c73\u9897\u7c92\u7684\u7535\u955c\u7167\u7247\uff1b<\/p>\n<p>\uff08c\uff09Pd\/Fe<sub>3<\/sub>O<sub>4<\/sub> \u6838\u58f3\u7eb3\u7c73\u9897\u7c92\u4ee5\u53ca\u6807\u6837\uff08Pd \u7247\uff09\u7684 XANES Pd K \u8fb9\u8c31\uff1b<\/p>\n<p>\uff08d\uff09Pd\/Fe<sub>3<\/sub>O<sub>4<\/sub> \u6838\u58f3\u7eb3\u7c73\u9897\u7c92\u4ee5\u53ca\u6807\u6837\uff08Fe3O4\u3001Fe2O3\uff09\u7684 XANES Fe K \u8fb9\u8c31\u3002<\/p>\n<p>\u56fe\u4e8c\uff1aPd\/FeO<sub>x<\/sub>(OH)<sub>2\u22122x<\/sub>\u7eb3\u7c73\u9897\u7c92\u7684\u8868\u9762\u8986\u76d6\u7387\u4ee5\u53ca\u5143\u7d20\u5206\u5e03\u8868\u5f81\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-97209 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/2-49.jpg\" alt=\"\" width=\"600\" height=\"708\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/2-49.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/2-49-254x300.jpg 254w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u4e0d\u540c\u5faa\u73af\u5708\u6570\u540e\u7684Pd\/FeO<sub>x<\/sub>(OH)<sub>2\u22122x<\/sub>\u7eb3\u7c73\u9897\u7c92\u7684CV\u66f2\u7ebf\uff1b<\/p>\n<p>\uff08b\uff09\u4e0d\u540c\u5faa\u73af\u5708\u6570\u540e\u7684Pd\/FeO<sub>x<\/sub>(OH)<sub>2\u22122x<\/sub>\u7eb3\u7c73\u9897\u7c92\u7684\u8868\u9762FeO<sub>x<\/sub>(OH)<sub>2\u22122x<\/sub>\u7684\u8986\u76d6\u7387\uff1b<\/p>\n<p>\uff08c\uff09Pd\/Fe3O4\u6838\u58f3\u7eb3\u7c73\u9897\u7c92\u7684\u9ad8\u5206\u8fa8\u7535\u955c\u4ee5\u53ca\u5143\u7d20\u5206\u5e03\u56fe\uff1b<\/p>\n<p>\uff08d\uff09Pd\/FeO<sub>x<\/sub>(OH)<sub>2\u22122x<\/sub>\u7eb3\u7c73\u9897\u7c92\u9ad8\u5206\u8fa8\u7535\u955c\u4ee5\u53ca\u5143\u7d20\u5206\u5e03\u56fe\u3002<\/p>\n<p>\u56fe\u4e09\uff1aPd\/FeO<sub>x<\/sub>(OH)<sub>2\u22122x<\/sub>\u7eb3\u7c73\u9897\u7c92\u539f\u4f4dXANES\u53caEXAFS\u8868\u5f81\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-97210 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/3-42.jpg\" alt=\"\" width=\"600\" height=\"590\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/3-42.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/3-42-300x295.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a)\u4e0d\u540c\u5faa\u73af\u5708\u6570\u540e\u7684Pd\/FeO<sub>x<\/sub>(OH)<sub>2\u22122x<\/sub>\u7eb3\u7c73\u9897\u7c92Fe-<em>K<\/em>\u8fb9\u7684\u539f\u4f4dXANES\u8c31\uff1b<\/p>\n<p>(b)\u4e0d\u540c\u5faa\u73af\u5708\u6570\u540e\u7684Pd\/FeO<sub>x<\/sub>(OH)<sub>2\u22122x<\/sub>\u7eb3\u7c73\u9897\u7c92Fe-<em>K<\/em>\u8fb9\u7684\u539f\u4f4dEXAFS k<sup>3<\/sup>\u03c7(R)\u8c31\uff1b<\/p>\n<p>(c)Pd\/FeO<sub>x<\/sub>(OH)<sub>2\u22122x<\/sub>\u7eb3\u7c73\u9897\u7c92Pd-<em>K<\/em>\u8fb9\u7684\u539f\u4f4dXANES\u548cEXAFS k<sup>3<\/sup>\u03c7(R)\u8c31\u3002<\/p>\n<p>\u56fe\u56db\uff1a\u4e0d\u540c\u5faa\u73af\u5708\u6570\u540e\u7684Pd\/FeO<sub>x<\/sub>(OH)<sub>2\u22122x<\/sub>\u7eb3\u7c73\u9897\u7c92\u7684\u7535\u5316\u5b66\u8868\u5f81<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-97211 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/4-36.jpg\" alt=\"\" width=\"600\" height=\"590\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/4-36.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/08\/4-36-300x295.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a)\u4e0d\u540c\u5faa\u73af\u5708\u6570\u540e\u7684Pd\/FeO<sub>x<\/sub>(OH)<sub>2\u22122x<\/sub>\u7eb3\u7c73\u9897\u7c92\u7684LSV\u66f2\u7ebf\uff1b<\/p>\n<p>(b)\u4e0d\u540c\u5faa\u73af\u5708\u6570\u540e\u7684Pd\/FeO<sub>x<\/sub>(OH)<sub>2\u22122x<\/sub>\u7eb3\u7c73\u9897\u7c92\u7684Tafel\u66f2\u7ebf\uff1b<\/p>\n<p>(c)\u4e0d\u540c\u5faa\u73af\u5708\u6570\u540e\u7684Pd\/FeO<sub>x<\/sub>(OH)<sub>2\u22122x<\/sub>\u7eb3\u7c73\u9897\u7c92\u7684TOF\u66f2\u7ebf\uff1b<\/p>\n<p>(d)HER\u6d3b\u6027\u4e0eFeO<sub>x<\/sub>(OH)<sub>2\u22122x<\/sub>\u8986\u76d6\u7387\u7684\u76f8\u5173\u56fe\u3002<\/p>\n<p><strong>\u3010\u5c0f\u7ed3\u3011<\/strong><\/p>\n<p>\u901a\u8fc7\u201c\u81ea\u4e0a\u800c\u4e0b\u201d\u7684\u7535\u5316\u5b66\u5faa\u73af\u8150\u8680\u7684\u65b9\u6cd5\u53ef\u63a7\u4fee\u9970Pd\u7eb3\u7c73\u9897\u7c92\u8868\u9762\u7684FeO<sub>x<\/sub>(OH)<sub>2\u22122x<\/sub>\u8986\u76d6\u7387\u3002Pd\/FeO<sub>x<\/sub>(OH)<sub>2\u22122x<\/sub>\u7eb3\u7c73\u7c92\u5b50\u5728\u78b1\u6027\u6761\u4ef6\u4e0b\u7684HER\u6d3b\u6027\u4e0e\u8868\u9762Fe(OH)<sub>2\u22122x<\/sub>\u8986\u76d6\u7387\u5448\u73b0\u51fa\u706b\u5c71\u5f62\u72b6\u7684\u5173\u7cfb\u3002\u5f53FeO<sub>x<\/sub>(OH)<sub>2\u22122x<\/sub>\u8986\u76d6\u7387\u8fbe\u523040%\u65f6\uff0c\u501f\u52a9\u4e8eFeO<sub>x<\/sub>(OH)<sub>2\u22122x<\/sub>\u89e3\u79bb\u6c34\u4ee5\u53caPd\u590d\u5408\u6c22\u7684\u534f\u540c\u4f5c\u7528\uff0c\u5176\u78b1\u6027\u6761\u4ef6\u4e0bHER\u6d3b\u6027\u53ef\u4ee5\u9ad8\u8fbe\u7eafPd\u7eb3\u7c73\u9897\u7c92\u768419\u500d\u4ee5\u4e0a\uff0cTOF\uff08\u8fc7\u7535\u52bf=150 mV\uff09\u662f\u7eafPd\u7eb3\u7c73\u9897\u7c92\u768425\u500d\u5de6\u53f3\u3002\u4e0d\u4ec5\u5982\u6b64\uff0c\u8fd9\u79cd\u201c\u591a\u4e2d\u5fc3\u201d\u7684\u7b56\u7565\u53ef\u4ee5\u5e94\u7528\u4e8e\u5176\u4ed6\u7c7b\u578b\u7684\u50ac\u5316\u5242\u5728\u78b1\u6027\u6761\u4ef6\u4e0bHER\u6027\u80fd\u7684\u4f18\u5316\u3002<\/p>\n<p>\u6587\u7ae0\u94fe\u63a5\uff1a<a href=\"http:\/\/onlinelibrary.wiley.com\/doi\/10.1002\/aenm.201701129\/abstract\" target=\"_blank\" rel=\"noopener\">A Multisite Strategy for Enhancing the Hydrogen Evolution Reaction on a Nano-Pd Surface in Alkaline Media<\/a>\uff08Advanced Energy Materials\uff0c2017\uff0cDOI: 10.1002\/aenm.201701129\uff09<\/p>\n<p>\u611f\u8c22\u5f90\u68bd\u5ddd\u6559\u6388\u56e2\u961f\u64b0\u6587\u4e0e\u652f\u6301\uff01\u6750\u6599\u4eba\u65b0\u80fd\u6e90\u7ec4\u80cc\u9006\u65f6\u5149\u6574\u7406\u7f16\u8f91\u3002<\/p>\n<p><strong>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1axiaofire-18\uff0c\u5434\u73ab\uff0c\u6211\u4eec\u4f1a\u9080\u8bf7\u5404\u4f4d\u8001\u5e08\u52a0\u5165\u4e13\u5bb6\u7fa4\u3002<\/strong><\/p>\n<p>\u6750\u6599\u725b\u7f51\u4e13\u6ce8\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u53ca\u884c\u4e1a\u8fdb\u5c55\uff0c\u5982\u679c\u60a8\u5bf9\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u8fdb\u5c55\uff0c\u89e3\u8bfb\u9ad8\u6c34\u5e73\u6587\u7ae0\u6216\u662f\u8bc4\u8ff0\u884c\u4e1a\u6709\u5174\u8da3\uff0c<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\" target=\"_blank\" rel=\"noopener noreferrer\">\u70b9\u6211\u52a0\u5165\u7f16\u8f91\u90e8<\/a>\u3002\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com\u3002<\/p>\n<p><strong>\u4eea\u5668\u8bbe\u5907\u3001\u8bd5\u5242\u8017\u6750\u3001\u6750\u6599\u6d4b\u8bd5\u3001\u6570\u636e\u5206\u6790\uff0c\u627e<\/strong><a href=\"http:\/\/mai.cailiaoren.com\/\" target=\"_blank\" rel=\"noopener noreferrer\"><strong>\u6750\u6599\u4eba<\/strong><\/a><strong>\u3001\u4e0a<\/strong><a href=\"http:\/\/www.ceshigu.com\/\" target=\"_blank\" rel=\"noopener noreferrer\"><strong>\u6d4b\u8bd5\u8c37<\/strong><\/a><strong>\uff01<\/strong><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u6790\u6c22\u53cd\u5e94\uff08HER\uff09\u662f\u6c34\u7535\u89e3\u7684\u9634\u6781\u53cd\u5e94\uff0c\u540c\u65f6\u4e5f\u662f\u4e00\u79cd\u7b80\u5355\u3001\u9ad8\u6548\u7684\u5236\u6c22\u65b9\u6cd5\u3002\u5de5\u4e1a\u6c34\u7535\u89e3\u5236\u6c22\u901a\u5e38\u662f\u572825\u201335% KOH\u78b1\u6027\u7535\u89e3\u6db2\u4e2d\u8fdb\u884c\u3002\u7136\u800c\uff0c\u7531\u4e8e\u78b1\u6027\u4ecb\u8d28&#8230;<\/p>\n","protected":false},"author":272,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[],"class_list":["post-97199","post","type-post","status-publish","format-standard","hentry","category-jiedu"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/97199"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/272"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=97199"}],"version-history":[{"count":2,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/97199\/revisions"}],"predecessor-version":[{"id":97213,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/97199\/revisions\/97213"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=97199"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=97199"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=97199"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}