{"id":99723,"date":"2017-09-04T06:30:30","date_gmt":"2017-09-03T22:30:30","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=99723"},"modified":"2017-09-01T17:49:23","modified_gmt":"2017-09-01T09:49:23","slug":"nature-%e5%ad%90%e5%88%8a%ef%bc%9a%e6%99%b6%e7%b2%92%e5%bc%82%e5%b8%b8%e9%95%bf%e5%a4%a7%e5%88%b6%e5%a4%87%e8%b6%85%e5%a4%a7%e5%8d%95%e6%99%b6","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=99723","title":{"rendered":"Nature \u5b50\u520a\uff1a\u6676\u7c92\u5f02\u5e38\u957f\u5927\u5236\u5907\u8d85\u5927\u5355\u6676"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/p>\n<p>\u5927\u90e8\u5206\u91d1\u5c5e\u3001\u9676\u74f7\u548c\u534a\u5bfc\u4f53\u6750\u6599\u90fd\u662f\u7531\u591a\u6676\u6784\u6210\u3002\u76f8\u6bd4\u4e4b\u4e0b\uff0c\u5355\u6676\u5c3d\u7ba1\u6027\u80fd\u5f80\u5f80\u66f4\u52a0\u4f18\u5f02\uff0c\u4f46\u76ee\u524d\u7531\u4e8e\u53d7\u6210\u672c\u9650\u5236\uff0c\u5176\u5e94\u7528\u8303\u56f4\u4ecd\u5341\u5206\u6709\u9650\uff0c\u65e0\u6cd5\u5b9e\u73b0\u5927\u89c4\u6a21\u751f\u4ea7\u3002\u4f20\u7edf\u7684\u5355\u6676\u5236\u5907\u6280\u672f\u5305\u62ecBridgeman\u6cd5\u548cCzochralski\u6cd5\u5728\u5185\u7684\u5b9a\u5411\u51dd\u56fa\u6cd5\uff0c\u6b64\u5916\uff0c\u4e5f\u53ef\u4ee5\u901a\u8fc7\u8bf1\u5bfc\u6676\u7c92\u5f02\u5e38\u957f\u5927\u7684\u65b9\u6cd5\u5408\u6210\u5355\u6676\u3002\u591a\u6676\u6750\u6599\u6676\u7c92\u957f\u5927\u901a\u5e38\u4ee5\u5927\u6676\u7c92\u201c\u541e\u566c\u201d\u5c0f\u6676\u7c92\u7684\u65b9\u5f0f\u8fdb\u884c\uff0c\u4ee5\u964d\u4f4e\u9ad8\u80fd\u6676\u754c\u7684\u767e\u5206\u6bd4\u3002\u5982\u679c\u6676\u7c92\u4ee5\u6b63\u5e38\u65b9\u5f0f\u957f\u5927\uff0c\u5219\u7c92\u5f84\u5206\u5e03\u76f8\u5bf9\u5747\u5300\uff1b\u7279\u5b9a\u60c5\u51b5\u4e0b\uff0c\u53ea\u6709\u90e8\u5206\u6676\u7c92\u201c\u541e\u566c\u201d\u5468\u56f4\u6676\u7c92\u800c\u5feb\u901f\u957f\u5927\uff0c\u8fd9\u79cd\u60c5\u51b5\u4fbf\u662f\u5f02\u5e38\u6676\u7c92\u957f\u5927\u3002\u622a\u6b62\u76ee\u524d\uff0c\u5355\u6676\u6750\u6599\u7684\u5e94\u7528\u5305\u62ec\u5f62\u72b6\u8bb0\u5fc6\u5408\u91d1\u548c\u8010\u70ed\u5408\u91d1\u7b49\u82e5\u5e72\u65b9\u9762\uff0c\u800c\u5f62\u72b6\u8bb0\u5fc6\u5408\u91d1\u4e2d\uff0c\u94dc-\u94dd-\u9530\u5408\u91d1\u5c24\u5176\u5177\u6709\u7a81\u51fa\u7684\u51b7\u52a0\u5de5\u6027\u3002\u6b64\u5916\u8fd9\u79cd\u5408\u91d1\u7684\u8d85\u5851\u6027\u968f\u7740\u6676\u7c92\u5c3a\u5bf8\u589e\u5927\u663e\u8457\u63d0\u9ad8\u3002\u56e0\u6b64\uff0c\u5982\u679c\u80fd\u5229\u7528\u4f20\u7edf\u70ed\u5904\u7406\u5b9e\u73b0\u94dc-\u94dd-\u9530\u5408\u91d1\u5355\u6676\u7684\u5927\u6279\u91cf\u5236\u5907\uff0c\u90a3\u4e48\u65e0\u7591\u4f1a\u5927\u5927\u63d0\u9ad8\u8be5\u5f62\u72b6\u8bb0\u5fc6\u5408\u91d1\u7684\u5e94\u7528\u524d\u666f\u3002<\/p>\n<p> <strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u8fd1\u65e5\u6765\uff0c<strong>\u65e5\u672c\u4e1c\u5317\u5927\u5b66<\/strong>\u7684<strong>Omori\u6559\u6388(\u901a\u8baf\u4f5c\u8005)\u7814\u7a76\u56e2\u961f<\/strong>\u5728<strong>Nature Communications<\/strong>\u4e0a\u53d1\u8868\u9898\u4e3a\u201c<strong>Ultra-large single crystals by abnormal grain growth<\/strong>\u201d\u7684\u6587\u7ae0\u3002\u8be5\u6587\u7ae0\u6307\u51fa\uff0c\u53ef\u4ee5\u901a\u8fc7\u4f20\u7edf\u70ed\u5904\u7406\u5de5\u827a\uff0c\u8bf1\u5bfc\u6676\u7c92\u5f02\u5e38\u957f\u5927\uff0c\u8fdb\u800c\u5b9e\u73b0\u94dc-\u94dd-\u9530\u5408\u91d1\u5355\u6676\u7684\u5927\u6279\u91cf\u5236\u5907\u3002\u5176\u4e2d\uff0c\u5faa\u73af\u70ed\u5904\u7406\u63d0\u4f9b\u4e86\u4f5c\u4e3a\u6676\u7c92\u5f02\u5e38\u957f\u5927\u4e3b\u8981\u9a71\u52a8\u529b\u7684\u4e9a\u6676\u754c\u80fd\uff1b\u800c\u8fdb\u4e00\u6b65\u7684\u5faa\u73af\u4f4e\u6e29\u70ed\u5904\u7406\u63d0\u9ad8\u4e86\u4e9a\u6676\u754c\u80fd\uff0c\u4ece\u800c\u63d0\u9ad8\u6676\u754c\u8fc1\u79fb\u901f\u7387\u3002\u901a\u8fc7\u8fd9\u6837\u7684\u70ed\u5904\u7406\uff0c\u80fd\u591f\u5b9e\u73b070\u5398\u7c73\u957f\u5355\u6676\u68d2\u7684\u5236\u5907\u3002\u8fd9\u4e00\u7814\u7a76\u6210\u679c\u4f7f\u5176\u5b83\u5177\u6709\u76f8\u4f3c\u7ed3\u6784\u7684\u91d1\u5c5e\u6216\u9676\u74f7\u6750\u6599\u7684\u5355\u6676\u5316\u6210\u4e3a\u53ef\u80fd\u3002\u6b64\u5916\uff0c\u7531\u4e8e\u76ee\u524d\u5355\u6676\u6750\u6599\u7684\u4e3b\u8981\u5e94\u7528\u4e4b\u4e00\u662f\u5f62\u72b6\u8bb0\u5fc6\u5408\u91d1\uff0c\u8fd9\u79cd\u5927\u6279\u91cf\u5236\u5907\u5355\u6676\u7684\u65b9\u6cd5\u4e5f\u5c06\u5927\u5927\u6269\u5c55\u73b0\u6709\u5f62\u72b6\u8bb0\u5fc6\u5408\u91d1\u7684\u5e94\u7528\u8303\u56f4\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p><strong>\u56fe\u4e00\uff1a\u94dc-\u94dd-\u9530\u5355\u6676\u68d2\u53ca\u70ed\u5904\u7406\u5de5\u827a<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-99724\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/1-1.jpg\" alt=\"\" width=\"600\" height=\"656\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/1-1.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/1-1-274x300.jpg 274w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>a.<\/strong>\u5faa\u73af\u70ed\u5904\u7406\u5de5\u827a\uff08\u9ad8\u6e29\u5faa\u73af\u7ed3\u5408\u4f4e\u6e29\u5faa\u73af\uff09<\/p>\n<p><strong>b.<\/strong>\u5faa\u73af\u70ed\u5904\u7406\u5de5\u827a\u5236\u5907\u7684\u94dc-\u94dd-\u9530\u5355\u6676\u68d2<\/p>\n<p><strong>c.<\/strong>\u4ec5\u9ad8\u6e29\u5faa\u73af\u70ed\u5904\u7406\u5de5\u827a<\/p>\n<p><strong>d.<\/strong>\u4ec5\u9ad8\u6e29\u5faa\u73af\u70ed\u5904\u7406\u5de5\u827a\u5236\u5907\u7684\u94dc-\u94dd-\u9530\u5355\u6676\u68d2<\/p>\n<p><strong>\u56fe\u4e8c\uff1a\u901a\u8fc7\u53cd\u5e38\u6676\u7c92\u957f\u5927\u5236\u5f97\u7684\u94dc-\u94dd-\u9530\u5408\u91d1\u7684\u5fae\u89c2\u5f62\u8c8c<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-99725\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/2-1.jpg\" alt=\"\" width=\"600\" height=\"1016\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/2-1.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/2-1-177x300.jpg 177w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n <strong>a.<\/strong>\u94dc-\u94dd-\u9530\u5408\u91d1\u81ea900\u2103\u5230500\u2103\u5faa\u73af\u7ed3\u675f\uff0c\u6dec\u706b\u540e\u7684\u5149\u5b66\u663e\u5fae\u955c\u7167\u7247<\/p>\n<p><strong>b.<\/strong>\u53cd\u6781\u56fe\u6295\u5f71<\/p>\n<p><strong>c.<\/strong>\u5404\u6676\u7c92\u7684\u53c2\u8003\u53d6\u5411\u504f\u5dee<\/p>\n<p><strong>\u56fe\u4e09\uff1a\u6676\u7c92\u5f02\u5e38\u957f\u5927\u73b0\u8c61<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-99726\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/3-1.jpg\" alt=\"\" width=\"600\" height=\"593\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/3-1.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/3-1-300x297.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>a.<\/strong>\u9ad8\u6e29\u5faa\u73af\u70ed\u5904\u7406\uff08900\/500\u2103\uff09\u8fc7\u7a0b\u4e2d\uff0c\u4e9a\u6676\u7c92\u7ed3\u6784\u5f62\u6210\uff0c\u90e8\u5206\u76f8\u5728500\u2103\u5f62\u6210\u6c89\u6dc0\u3002\u5faa\u73af\u70ed\u5904\u7406\u540e\uff0c\u90e8\u5206\u6676\u7c92\u5728\u4e9a\u6676\u754c\u80fd\u7684\u9a71\u52a8\u4e0b\u5f02\u5e38\u957f\u5927<\/p>\n<p><strong>b.<\/strong>\u591a\u6b21\u4f4e\u6e29\u5faa\u73af\u70ed\u5904\u7406\uff08740\/500\u2103\uff09\u540e\uff0c\u7531\u4e8e\u4e9a\u6676\u7c92\u4e4b\u95f4\u53d6\u5411\u5dee\u589e\u5927\uff0c\u56e0\u6b64\u4e9a\u6676\u754c\u80fd\u5347\u9ad8\uff0c\u6676\u754c\u8fc1\u79fb\u901f\u7387\u589e\u5927\uff0c\u4e3a\u8d85\u5927\u6676\u7c92\u7684\u5b9e\u73b0\u63d0\u4f9b\u53ef\u80fd<\/p>\n<p><strong>\u56fe\u56db\uff1a\u6676\u754c\u8fc1\u79fb\u8ddd\u79bb\u548c\u4e9a\u6676\u7c92\u7ed3\u6784<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-99727\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/4-1.jpg\" alt=\"\" width=\"600\" height=\"619\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/4-1.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/4-1-291x300.jpg 291w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>a.<\/strong>\u5408\u91d1\u5728800-500-800\u2103\u4e2d\u6e29\u5faa\u73af\u540e\uff0c\u5728800\u2103\u5206\u522b\u4fdd\u6e29\u4e00\u5b9a\u65f6\u95f4\uff080min, 5min,10min\uff09\u5e76\u6dec\u706b\u5f62\u6210\u7684\u663e\u5fae\u7ec4\u7ec7<\/p>\n<p><strong>b.<\/strong>\u5408\u91d1\u5728740-500-740\u2103\u4e2d\u6e29\u5faa\u73af\u4e94\u6b21\uff0c\u5728800\u2103\u5206\u522b\u4fdd\u6e29\u4e00\u5b9a\u65f6\u95f4\uff080min, 2min,10min\uff09\u5e76\u6dec\u706b\u5f62\u6210\u7684\u663e\u5fae\u7ec4\u7ec7<\/p>\n<p><strong>c.<\/strong>\u5f02\u5e38\u6676\u7c92\u7684\u6676\u754c\u8fc1\u79fb\u8ddd\u79bb<\/p>\n<p><strong>d.<\/strong>\u6676\u7c92\u53c2\u8003\u53d6\u5411\u504f\u5dee<\/p>\n<p><strong>e.<\/strong>\u4e0e\u4e00\u6b21\u548c\u4e94\u6b21\u4f4e\u6e29\u5faa\u73af\u540e\u7684\u53d6\u5411\u504f\u5dee<\/p>\n<p><strong>\u56fe\u4e94:\u5355\u6676\u68d2\u7684\u8d85\u5851\u6027\u6d4b\u8bd5<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-99729\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/6.jpg\" alt=\"\" width=\"600\" height=\"440\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/6.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/6-300x220.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p style=\"text-align: center;\">\u76f4\u5f8415.4mm, \u957f682mm\u94dc-\u94dd-\u9530\u5355\u6676\u68d2\u7684\u8d85\u5851\u6027\u6d4b\u8bd5<\/p>\n<p><strong>\u3010\u5c0f\u7ed3\u3011<\/strong><\/p>\n<p>\u672c\u6587\u901a\u8fc7\u5408\u7406\u8bbe\u8ba1\u5408\u91d1\u7684\u70ed\u5904\u7406\u5de5\u827a\uff0c\u5b9e\u73b0\u4e86\u94dc-\u94dd-\u9530\u5408\u91d1\u7684\u8d85\u5927\u5355\u6676\u5236\u5907\u3002\u9996\u5148\u901a\u8fc7\u4e94\u6b21900-500\u2103\u9ad8\u6e29\u5faa\u73af\uff0c\u5728\u5408\u91d1\u4e2d\u5f62\u6210\u7c7b\u7af9\u8282\u7ed3\u6784\uff0c\u4e4b\u540e\u901a\u8fc7\u56db\u6b21740-500\u2103\u4f4e\u6e29\u5faa\u73af\uff0c\u83b7\u5f97\u6676\u754c\u8fc1\u79fb\u9a71\u52a8\u529b\uff0c\u5b9e\u73b0\u7c7b\u7af9\u8282\u7684\u5f02\u5e38\u957f\u5927\u3002\u8fd9\u4e00\u5de5\u827a\u5236\u5f97\u7684\u957f700mm\uff0c\u76f4\u5f84\u4e3a15mm\u7684\u5355\u6676\u68d2\u5177\u6709\u826f\u597d\u7684\u8d85\u5851\u6027\u3002\u6b64\u5916\uff0c\u8be5\u5b9e\u9a8c\u601d\u8def\u4e3a\u5b9e\u73b0\u5355\u6676\u7684\u5927\u6279\u91cf\u751f\u4ea7\u63d0\u4f9b\u4e86\u53ef\u80fd\uff0c\u62d3\u5bbd\u4e86\u5f62\u72b6\u8bb0\u5fc6\u5408\u91d1\u7684\u5e94\u7528\u524d\u666f\u3002\u9664\u94dc-\u94dd-\u9530\u5408\u91d1\u5916\uff0c\u540c\u6837\u5177\u6709\u6676\u7c92\u5f02\u5e38\u957f\u5927\u73b0\u8c61\u7684\u94dc-\u950c\uff0c\u94c1-\u94ec-\u94b4-\u94bc\u548c\u94c1-\u9530-\u94dd-\u954d\u5408\u91d1\u4e5f\u6709\u671b\u901a\u8fc7\u6b64\u5de5\u827a\u5b9e\u73b0\u5355\u6676\u7684\u5927\u6279\u91cf\u751f\u4ea7\u3002<\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5\uff1a<\/strong><a href=\"https:\/\/www.nature.com\/articles\/s41467-017-00383-0\" target=\"_blank\" rel=\"noopener\">Ultra-large single crystals by abnormal grain growth<\/a>\u00a0\uff08Nat. Commun. 2017,8,354, doi: 10.1038\/s41467-017-00383-0\uff09<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u7f16\u8f91\u90e8\u9ec4\u5b50\u82b8\u7f16\u8bd1\uff0c\u9648\u70b3\u65ed\u5ba1\u6838\uff0c<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\" target=\"_blank\" rel=\"noopener\">\u70b9\u6211\u52a0\u5165\u6750\u6599\u4eba\u7f16\u8f91\u90e8<\/a>\u3002<\/p>\n<p><strong>\u6750\u6599\u6d4b\u8bd5\uff0c\u6570\u636e\u5206\u6790\uff0c\u4e0a<a href=\"http:\/\/www.ceshigu.com\/\" target=\"_blank\" rel=\"noopener\">\u6d4b\u8bd5\u8c37<\/a>\uff01<\/strong><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u5927\u90e8\u5206\u91d1\u5c5e\u3001\u9676\u74f7\u548c\u534a\u5bfc\u4f53\u6750\u6599\u90fd\u662f\u7531\u591a\u6676\u6784\u6210\u3002\u76f8\u6bd4\u4e4b\u4e0b\uff0c\u5355\u6676\u5c3d\u7ba1\u6027\u80fd\u5f80\u5f80\u66f4\u52a0\u4f18\u5f02\uff0c\u4f46\u76ee\u524d\u7531\u4e8e\u53d7\u6210\u672c\u9650\u5236\uff0c\u5176\u5e94\u7528\u8303\u56f4\u4ecd\u5341\u5206\u6709\u9650\uff0c\u65e0\u6cd5\u5b9e\u73b0\u5927\u89c4\u6a21\u751f\u4ea7\u3002\u4f20\u7edf\u7684&#8230;<\/p>\n","protected":false},"author":230,"featured_media":99728,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215,2],"tags":[293,54],"class_list":["post-99723","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-jiedu","category-keji","tag-nature","tag-making"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/99723"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/230"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=99723"}],"version-history":[{"count":4,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/99723\/revisions"}],"predecessor-version":[{"id":99792,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/99723\/revisions\/99792"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/99728"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=99723"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=99723"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=99723"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}